Electrophoretic particle, electronic ink and application thereof
By using metal organic framework materials (MOFs) to wrap chromogenic particles, the problem of particle agglomeration and mutual repulsion in electronic paper is solved, the display stability and effect are improved, the preparation process is simplified and the cost is reduced, and the market of electronic paper is improved. competitiveness.
Patent Information
- Application Number
- CN202410765310.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-15
Smart Images

Figure HDA0004892595390000011 
Figure HDA0004892595390000012 
Figure HDA0004892595390000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrophoretic display, and in particular to an electrophoretic particle, electronic ink and applications thereof. Background Art
[0002] Electronic paper technology is a display technology that can achieve comfortable reading like paper, ultra-thin, light, bendable, and ultra-low power consumption. Electronic paper has low power consumption and foldable and bendable functions, with delicate display and wide viewing angle. Compared with other display technologies, its biggest advantage is good visibility in sunlight without blind spots. At present, electronic paper technology has stood out from many display technologies and has become one of the most promising flexible electronic display technologies.
[0003] Electronic paper generally uses electrophoretic display technology, and its display principle is that charged electrophoretic particles of different colors move under the action of an electric field to display the desired pattern. However, during the display process, due to the principle that unlike charges attract and like charges repel, charged particles of different electrical properties tend to agglomerate, and charged particles of the same electrical property repel each other during the display process, resulting in a decrease in the display effect.
[0004] At present, the above problems are generally solved by grafting polymers on the surface of electrophoretic particles, which makes the preparation process of electrophoretic particles very complicated. Take the preparation of black particles as an example: it is necessary to first coat the black particles with tetraethylsiloxane (TEOS) and add a small amount of silane coupling agent, and form a polymerization starting point through the reaction of the exposed amino group with the bromine-substituted acyl bromide. Then, through free radical polymerization, the monomer DMAEMA is chemically bonded to the particles to provide sites for generating positive charges. Then, DEGDMA (or other structures that can generate cross-linking) is polymerized on the particles to form a polymer protective layer to generate steric hindrance. Then, a charge control agent is added to form a reverse micelle to separate positive and negative ions and make the particles charged.
[0005] The above multi-step reactions are not only cumbersome, but also result in very low reaction yields, which directly leads to higher costs for electronic paper and affects its market application prospects. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide an electrophoretic particle, electronic ink and application thereof, which solves the problem of electrophoretic particle agglomeration and improves the display effect of the electronic ink.
[0007] The present invention provides an electrophoretic particle, comprising a color-developing particle and a coating layer, wherein the coating layer wraps the color-developing particle, wherein the coating layer comprises a MOFs material.
[0008] The invention provides an electronic ink, comprising the electrophoretic particles mentioned above.
[0009] The present invention provides an electronic ink display device, comprising a first substrate and a second substrate, and an electronic ink layer disposed between the first substrate and the second substrate;
[0010] The electronic ink layer includes the electronic ink mentioned above.
[0011] Compared with the prior art, the present invention can prevent the mutual attraction between particles of the same charge or the mutual repulsion between particles of different charges by fixing the color-developing particles in the MOFs material, and helps to maintain the stability of the charge of the particles, thereby improving the driving stability of the electronic paper display, improving the display effect, and bringing consumers a better reading experience. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 is the transmission electron microscopy image of the modified black particles;
[0013] Figure 2 The transmission electron microscope image of ZIF-8 prepared by the present invention;
[0014] Figure 3 Transmission electron microscopy image of ZIF-8 and modified black particles after assembly. DETAILED DESCRIPTION
[0015] The present invention provides an electrophoretic particle, comprising a color-developing particle and a coating layer, wherein the coating layer wraps the color-developing particle, wherein the coating layer comprises a MOFs material.
[0016] The above-mentioned MOFs material refers to the metal organic framework material well known to those skilled in the art. The present invention uses MOFs material as a wrapping material for color-developing particles, which can achieve the loading and effective confinement of the color-developing particles. The color-developing particles are wrapped by MOFs material so that the distance between adjacent color-developing particles cannot be too close, and cannot form agglomeration or repulsion.
[0017] Optionally, the MOFs materials include but are not limited to any one or more of reticular metal organic framework materials IRMOF, zeolite-imidazole framework materials ZIF, Levahill organic framework materials MIL, and channel framework materials PCN, etc. Zeolite-imidazole framework materials ZIF are preferred.
[0018] Experimental studies have shown that ZIF materials are more compatible with color-developing particles, which is beneficial for reducing the agglomeration or repulsion of color-developing particles, and is not easy for particles to escape, thus having higher stability.
[0019] The present invention has no particular limitation on the preparation method of the above MOFs material, and it can be a method well known to those skilled in the art.
[0020] The present invention performs a modification pre-treatment on the color-developing particles before encapsulation, so that the color-developing particles can more easily enter the interior of the MOFs material.
[0021] Optionally, the above-mentioned pre-modification treatment includes: coating the surface of the color-developing particles with a silica coating; and grafting positively or negatively charged groups on the surface of the silica coating.
[0022] The present invention has no particular limitation on the method for preparing the silicon dioxide coating, and the method may be a method well known to those skilled in the art.
[0023] In some specific embodiments of the present invention, the color-developing particles and the sodium silicate solution are reacted in water to form a silicon dioxide coating on the surface of the color-developing particles.
[0024] Optionally, the above-mentioned positively or negatively charged group is a salt of N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine with positive or negative charge, including but not limited to sodium sulfate salt, hydrochloride, etc.
[0025] The above modification is achieved by adding easily leaving groups to the surface of the color-developing particles to form chargeability.
[0026] The present invention adopts the above-mentioned modification method to make the color-developing particles wrapped by MOFs materials. The reaction process is simple to operate and has a high yield. There is no need for complicated treatment of surface grafted polymers, which greatly reduces the difficulty and cost of preparing the color-developing particles, thereby effectively reducing the production cost of electronic paper, making it more competitive in the market. This technology has broad market application prospects.
[0027] The color-developing particles used in the present invention have at least two different colors, including but not limited to black, white, or yellow, green, blue and other colored particles, so that the display device prepared with the color-developing particles can display black and white or color.
[0028] Optionally, the color-developing particles include first color-developing particles.
[0029] Optionally, the first color-developing particle includes a particle surface modified with N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine sodium sulfate or hydrochloride.
[0030] Optionally, the particle size of the first color-developing particles is 100 to 500 nm.
[0031] In some specific embodiments of the present invention, the first color-developing particles are black particles.
[0032] Optionally, the black particles are modified carbon black particles.
[0033] Optionally, the surface of the modified carbon black particles is coated with a silicon dioxide coating, and then grafted with N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine sodium sulfate or hydrochloride.
[0034] Optionally, the color-developing particles include first color-developing particles and second color-developing particles, and the first color-developing particles and the second color-developing particles have different colors; wherein the particle size of the first color-developing particles is smaller than that of the second color-developing particles.
[0035] Optionally, the surface of the second color-developing particle is modified with N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine hydrochloride or sodium sulfate.
[0036] Optionally, the particle size of the second color-developing particles is 300-500 nm.
[0037] In some specific embodiments of the present invention, the second color-developing particles are white particles.
[0038] Optionally, the second color-developing particles are modified titanium dioxide particles.
[0039] Optionally, the surface of the modified titanium dioxide particles is coated with a silicon dioxide coating, and then grafted with N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine hydrochloride or sodium sulfate.
[0040] The first color-developing particles and the second color-developing particles have different surface electrical properties.
[0041] For the purpose of improving the compatibility between the color-developing particles and MOFs materials, the present invention optionally comprises: the coating layer corresponding to the first color-developing particles comprises a ZIF-8 metal organic framework material; and the coating layer corresponding to the second color-developing particles is a ZIF-L metal organic framework material.
[0042] Optionally, the ZIF-8 metal organic framework material has a first pore.
[0043] Optionally, the diameter of the first pore is 110-120 nm.
[0044] This diameter range helps the ZIF-8 metal organic framework material to better wrap the first color-developing particles and prevent them from escaping easily.
[0045] Optionally, the ZIF-L metal organic framework material has a second pore.
[0046] Optionally, the diameter of the second pore is 360-390 nm.
[0047] This diameter range helps the ZIF-L metal organic framework material to better wrap the second color-developing particles and prevent them from escaping easily.
[0048] Optionally, the number of the first pores is 1 to 12.
[0049] Optionally, the number of the second pores is 1 to 8.
[0050] The above-mentioned limitation of the number of pores helps to regulate the number of loaded color-developing particles.
[0051] Optionally, the ZIF-8 metal organic framework material is prepared according to the following method:
[0052] The metal source compound and 2-methylimidazole were stirred and reacted in a methanol solvent to separate the MOFs material ZIF-8;
[0053] The stirring reaction time is 18 to 22 minutes.
[0054] Optionally, the metal source compound is a zinc-containing compound or a cobalt-containing compound, preferably zinc nitrate or zinc nitrate hexahydrate.
[0055] Optionally, the molar ratio of the metal source compound to 2-methylimidazole is 1:(7-8).
[0056] After the reaction is completed, preferably, the precipitate is centrifuged and the obtained separated product is washed and dried to obtain a suitable ZIF-8 metal organic framework material.
[0057] Optionally, the ZIF-L metal organic framework material is prepared according to the following method:
[0058] The metal source compound and 2-methylimidazole were stirred and reacted in water to separate the MOFs material ZIF-L;
[0059] The stirring reaction time is 27 to 33 minutes.
[0060] Optionally, the metal source compound is a zinc-containing compound or a cobalt-containing compound, preferably zinc nitrate or zinc nitrate hexahydrate.
[0061] Optionally, the molar ratio of the metal source compound to 2-methylimidazole is 1:(7-8).
[0062] After the reaction is completed, preferably, the precipitate is centrifuged and the obtained separated product is washed and dried to obtain a suitable ZIF-L metal organic framework material.
[0063] The present invention is aimed at different color-developing particles, and by controlling the stirring time and the feeding amount of the metal source compound and 2-methylimidazole, the ZIF-8 and ZIF-L metal organic framework materials respectively form the pore size and pore number that meet the requirements. Among them, the appropriate pore size enables it to be better adapted to the color-developing particles, can accommodate the color-developing particles, and can form a certain restriction on the particles, and prevent too many particles from entering and exiting the MOFs material during use, thereby improving the stability of the display. The appropriate number of pores is also very critical. The more the number of pores, the larger the volume of the MOFs skeleton, so that the viscous resistance of MOFs in the electrophoretic solution will increase more, resulting in a slower particle response time; if the number of pores is too small, the amount of particles carried by the unit MOFs will be reduced, and the mass ratio of MOFs in the entire particle group will be increased, resulting in a reduction in the thrust-to-weight ratio of the driving force of the charge action to the mass of the group, which is not conducive to particle movement.
[0064] The above different color-developing particles respectively wrapping different MOFs materials is the optimal technical solution of the present invention. As a generally feasible solution, only the first color-developing particle wraps the MOFs material, or only the second color-developing particle wraps the MOFs material, which can also achieve the technical effect of avoiding particle agglomeration or repulsion, and should be included in the protection scope of the present invention as a general replacement solution.
[0065] In some specific embodiments of the present invention, only the first color-developing particles wrap the MOFs material, preferably the ZIF-8 metal organic framework material.
[0066] In some other specific embodiments of the present invention, only the second color-developing particles wrap the MOFs material, preferably the ZIF-L metal organic framework material.
[0067] For color development technology, color development particles of various colors can be included, so more MOFs materials are needed, and their corresponding technical solutions should also be included in the protection scope of the present invention as general replacement solutions.
[0068] In the present invention, the amount of MOFs material added is based on ensuring that the total number of pores in the system is greater than the total number of color-developing particles. If the number of pores is insufficient, MOFs material can be added to ensure that all color-developing particles are coated with MOFs material.
[0069] Optionally, the mass ratio of the MOFs material to the color-developing particles is 1:0.5-20, preferably 1:5.
[0070] Optionally, the step of wrapping the color-developing particles with the MOFs material is as follows:
[0071] The MOFs material and the color-developing particles are mixed in a plasma solvent to achieve encapsulation of the color-developing particles and the MOFs material.
[0072] The present invention has no particular limitation on the above-mentioned plasma solvent, and it can be any plasma solvent well known to those skilled in the art.
[0073] Optionally, the plasma solvent is a C7-C15 isoalkane, including but not limited to C13-15 alkane, C10-13-isoalkane, etc.
[0074] Optionally, during the above mixing process, the system also includes a charge generator to make the color-developing particles have electrical properties.
[0075] The present invention has no particular limitation on the charge generating agent, and the charge generating agent may be any charge generating agent known to those skilled in the art.
[0076] Optionally, the charge generating agent includes but is not limited to sodium dodecylbenzene sulfonate, Triton TM X-100, etc.
[0077] Optionally, the concentration of the charge generating agent in the system is 0.1 wt% to 1 wt%, preferably 0.1 wt%.
[0078] The invention provides an electronic ink, comprising the electrophoretic particles mentioned above.
[0079] The present invention provides an electronic ink display device, comprising a first substrate and a second substrate, and an electronic ink layer disposed between the first substrate and the second substrate;
[0080] The electronic ink layer includes the electronic ink mentioned above.
[0081] To further illustrate the present invention, the electrophoretic particles, electronic ink and their applications provided by the present invention are described in detail below in conjunction with the embodiments. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention.
[0082] All raw materials of the present invention have no particular limitation on their sources, and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0083] Example 1
[0084] 1. Black particle modification:
[0085] Black 1G (50 g) from Xuegao Pigment Company, water (420 mL) and sodium silicate solution (6 mL of solution containing 14% sodium hydroxide and 27% silicon dioxide) were fully mixed and ultrasonicated for one hour and then added to a three-necked flask. The three-necked flask was placed in an oil bath and gradually heated to 100°C while stirring vigorously. After reaching 100°C, 0.22M sulfuric acid (70 mL) and 11 mL of the aforementioned sodium silicate solution and water (70 mL) were gradually added and stirred for 2 hours, then cooled and centrifuged to obtain a black solid. The black solid was ground into powder.
[0086] The above product was rapidly stirred for 5 minutes in 300 mL of ethanol, 30 mL of water and 40 g of a 40% by mass fraction of N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine hydrochloride methanol solution. The above mixture was stirred and centrifuged, and then dried at 70°C.
[0087] The modified black particles were tested by scanning electron microscopy, and the results were as follows: Figure 1 shown.
[0088] After testing, the modified black particles have a non-standard spherical morphology and a particle size of 80-150nm.
[0089] 2. Preparation of ZIF-8:
[0090] Dissolve 0.1 mol of zinc nitrate in 2 L of methanol to obtain a zinc nitrate methanol solution; dissolve 0.79 mol of 2-methylimidazole in 2 L of methanol to obtain a 2-methylimidazole methanol solution. Mix the two solutions together and stir at room temperature for 20 minutes. Centrifuge the obtained precipitate at 4000 rpm for 10 minutes. Wash the obtained isolate with methanol three times, then dry the product in the atmosphere for 16 hours, and then dry it under vacuum at 50°C for 12 hours.
[0091] The obtained ZIF-8 was examined by scanning electron microscopy, and the results were as follows: Figure 2 shown.
[0092] Depend on Figure 2 It can be seen that the prepared ZIF-8 material has holes.
[0093] 3. Assembly:
[0094] In a container containing 1L of plasma solvent isoparaffin C7-C15, the ZIF-8 encapsulating agent prepared in step 2 was added, followed by 20g of the modified black particles and 0.1mol of the charge generating agent sodium dodecylbenzene sulfonate. The obtained plasma solution was stirred at room temperature at a speed of 30 rpm for 30 minutes to achieve encapsulation of black particles and ZIF-8.
[0095] The assembled particles were examined by scanning electron microscopy, and the results were as follows: Figure 3 shown. Figure 3 In the figure, the red arrow indicates the hole location, and the blue arrow indicates the encapsulated black particles.
[0096] Depend on Figure 3 You can see the original images of different MOFs single crystal groups ( Figure 2 ) The gray part is adsorbed with black particles and the original holes are filled, which indicates that the black particles are encapsulated in the pores of the ZIF-8 encapsulant.
[0097] Performance Testing
[0098] Using ITO glass with a film thickness of 100 nm, the electrophoretic liquid was filled into the space between two ITO glasses with a face-to-face distance of 20 microns, and an alternating electric field with an amplitude of ±15V and a period of 2 seconds was applied to the two ITO glasses. The electrophoretic liquids were respectively the black / white particles wrapped with MOF prepared in Example 1-2 and the conventional black / white particles not wrapped with MOF prepared in Comparative Example 1-2.
[0099] The test method is to use Konica Minolta's CA410 color analyzer, calibrate the light source to 1000nits, and test the maximum and minimum brightness changes of the ITO glass surface under the aforementioned alternating electric field. The brightness changes are recorded as follows.
[0100] Table 1
[0101] time 1 minute 1 hour 2 hours 5 hours 24 hours 48 hours 72 hours Example 2 400 396 390 388 382 383 381 Example 1 15 16 19 21 22 22 22 Comparative Example 2 380 350 330 320 319 322 318 Comparative Example 1 16 22 25 26 25 26 27
[0102] It can be seen that after 72 hours, the brightness of the white particles of the color-developing particle plasma material wrapped with MOFs provided by the present invention only decreased by 19 nits, and the brightness of the black particles only increased by 7 nits, achieving a good effect.
[0103] Example 2, White Particle Modification:
[0104] The white titanium dioxide particles were modified using the same method as in Example 1.
[0105] 2. Preparation of ZIF-L:
[0106] Dissolve 0.089 mol of zinc nitrate hexahydrate in 190 ml of water to obtain a zinc nitrate aqueous solution; dissolve 0.64 mol of 2-methylimidazole in 1.8 L of water. Mix the two solutions together and stir at room temperature for 30 minutes. Then separate the precipitate using a centrifuge at 4000 rpm for 10 minutes. Wash the precipitate with water three times, then dry the product in the atmosphere for 16 hours, and then dry it under vacuum at 50°C for 12 hours.
[0107] 3. Assembly:
[0108] In a container containing 1L of plasma solvent isoalkane C7-C15 (, add the ZIF-L encapsulating agent prepared above, then add 20g of the modified white particles above, and add 0.1mol of the charge generator (please provide the specific substance of the charge generator). The obtained plasma solution was stirred at room temperature at a speed of 30rpm for 30min to achieve the encapsulation of white particles and ZIF-L.
[0109] Comparative Example 1
[0110] 1. Black particle modification:
[0111] Black 1G from Xuegao Pigment Company was used, and the modification method was described in reference to US20050000813A1, Examples 1 to 3.
[0112] The prepared modified particles were subjected to the same performance tests as in Example 1, and the results are shown in Table 1.
[0113] Comparative Example 2
[0114] The same white titanium dioxide particles as in Example 2 were used, and the modification method was described in US 20050000813A1, Examples 1 to 3.
[0115] The prepared modified particles were subjected to the same performance tests as in Example 1, and the results are shown in Table 1.
[0116] It can be seen that the present application achieves higher stability by encapsulating the color-developing particles through MOFs.
[0117] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. An electrophoretic particle, It is characterized in that It comprises color-developing particles and a coating layer, wherein the coating layer wraps the color-developing particles, wherein the coating layer comprises MOFs material.
2. The electrophoretic particle according to claim 1, It is characterized in that The material of the coating layer is selected from any one or more of a reticular metal organic framework material IRMOF, a zeolite-imidazole framework material ZIF, a Levahill organic framework material MIL and a channel framework material PCN.
3. The electrophoretic particle according to claim 1, It is characterized in that The color-developing particles include first color-developing particles, and the surface of the first color-developing particles is modified with a group with a positive charge or a negative charge; The positively or negatively charged group is selected from a salt of positively or negatively charged N-[3-(trimethoxysilyl)propyl]-N′-(4-vinylbenzyl)ethylenediamine; The salt is selected from sodium sulfate salt or hydrochloride salt.
4. The electrophoretic particle according to claim 1, It is characterized in that The color-developing particles include first color-developing particles and second color-developing particles, and the first color-developing particles and the second color-developing particles have different colors; wherein the particle size of the first color-developing particles is smaller than that of the second color-developing particles.
5. The electrophoretic particle according to claim 4, It is characterized in that The particle size of the first color-developing particle is 100 to 500 nm; The particle size of the second color-developing particles is 300-500 nm.
6. The electrophoretic particle according to claim 1, It is characterized in that The color-developing particles include a first color-developing particle and a second color-developing particle, and the coating layer corresponding to the first color-developing particle includes a ZIF-8 metal organic framework material; The coating layer corresponding to the second color-developing particles is a ZIF-L metal organic framework material.
7. The electrophoretic particle according to claim 6, It is characterized in that The ZIF-8 metal organic framework material has a first pore; The diameter of the first pore is 110-120 nm; The ZIF-L metal organic framework material has a second pore; The diameter of the second pore is 360-390 nm.
8. The electrophoretic particle according to claim 7, It is characterized in that The number of the first pores is 1 to 12; The number of the second pores is 1 to 8.
9. The electrophoretic particle according to any one of claims 6 to 8, It is characterized in that The ZIF-8 metal organic framework material is prepared according to the following method: The metal source compound and dimethylimidazole were stirred and reacted in a methanol solvent to separate the MOFs material ZIF-8; The stirring reaction time is 18 to 22 minutes.
10. The electrophoretic particle according to any one of claims 6 to 8, It is characterized in that The ZIF-L metal organic framework material is prepared according to the following method: The metal source compound and dimethylimidazole were stirred and reacted in water to separate the MOFs material ZIF-L; The stirring reaction time is 27 to 33 minutes.
11. An electronic ink comprising any of the electrophoretic particles described above.
12. An electronic ink display device, comprising a first substrate and a second substrate, and an electronic ink layer disposed between the first substrate and the second substrate; The electronic ink layer includes the electronic ink according to claim 11.
Citation Information
Patent Citations
Electrophoretic particles, and processes for the production thereof
US20050000813A1