Lithium ion secondary battery electrolyte and application thereof

By using additives containing unsaturated bonds and nitrogen atoms in the electrolyte of lithium-ion secondary batteries, the gas production problem of high-nickel cathode materials is solved, the safety performance and initial dynamics of the battery are improved, and more efficient lithium-ion batteries are achieved. Secondary battery performance.

CN118782907APending Publication Date: 2024-10-15ENVISION AESC JAPAN LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410909975.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

High-nickel cathode materials have serious gas production in lithium-ion secondary batteries, leading to battery expansion and safety hazards. Existing solutions are not effective in energy density and initial power.

Method used

A lithium-ion secondary battery electrolyte is used, which contains a non-aqueous solvent, a lithium salt and a specific additive. The additive complexes transition metal ions through unsaturated bonds and nitrogen atoms, preventing them from dissolving and neutralizing H+ in the system, thereby improving Safety performance and initial dynamics of batteries.

Benefits of technology

Effectively prevent the dissolution of transition metal ions, prevent internal short circuits, improve initial kinetics, reduce HF content, and improve the safety and performance of lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118782907A_ABST
    Figure CN118782907A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion secondary battery electrolyte and an application thereof. The electrolyte comprises: a non-aqueous solvent; a lithium salt; the additive comprises a compound represented by any one of formulas (I)-(III): # imgabs 0 # # imgabs 1 #, R1, R2, R3, R4, R5, R6 and R7 are substituent groups with the carbon atom number of 1-3, the heteroatom number of 0-3 and the unsaturation degree of 0-4 respectively, and R1, R2, R3, R4, R5, R6 and R7 are substituent groups with the carbon atom number of 1-3, the heteroatom number of 0-3 and the unsaturation degree of 0-4 respectively; r8 is a cyclic substituent group with the unsaturation degree of 0-4, the number of heteroatoms is 0-5, when the unsaturation degree of R8 is 0, R9 is vinyl, allyl, butenyl, 1, 3-butadienyl, ethynyl and propynyl, and when the unsaturation degree of R8 is 1-4, the substituent group of R9 does not exist; heteroatoms are selected from at least one of nitrogen, fluorine and oxygen, and n is 0-2. According to the lithium ion secondary battery electrolyte and the application thereof provided by the invention, the dissolution of transition metal ions on the positive electrode side can be prevented, the problems of initial kinetics and gas production are improved, and the performance of a lithium ion secondary battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of power batteries, and in particular to a lithium-ion secondary battery electrolyte and applications thereof. Background Art

[0002] As the demand for electric vehicles and portable devices continues to grow, the development of lithium-ion secondary batteries is also changing with each passing day. In commercial lithium-ion secondary batteries, the positive electrode material accounts for more than 50% of the total mass and cost, and thus becomes a key factor in determining the energy density and cost of lithium-ion secondary batteries.

[0003] Among many positive electrode materials, high nickel positive electrode materials have the potential to achieve high energy density, are mature in development, and have a considerable cycle life. However, due to the decomposition reaction of lithium-related compounds in the battery, the side reactions between the shell and the acidic environment of the system, the oxidation reaction between the electrolyte and the high nickel positive electrode, or the dissolution of transition metal ions in the positive electrode material, high nickel positive electrode materials have serious gas production. The accumulation of gas can cause battery expansion, mechanical failure of the battery shell, and even battery explosion, so there are certain hidden dangers in safety performance. In order to solve the high-temperature gas production of high nickel positive electrode materials, the main methods used are material coating, adding positive electrode film-forming additives, transition metal ion trapping agents or stabilizers, but there are problems with energy density, initial power, and poor effect on the battery system. Summary of the invention

[0004] The present invention proposes a lithium ion secondary battery electrolyte and its application. The lithium ion secondary battery electrolyte provided by the present invention and its application can prevent the dissolution of transition metal ions on the positive electrode side, prevent the transition metal ions from diffusing to the negative electrode and causing internal short circuit, and at the same time improve the initial kinetics, neutralize the H generated by the system. + , improve the gas production problem of lithium-ion secondary batteries and improve the performance of lithium-ion secondary batteries.

[0005] In order to solve the above technical problems, the present invention provides a lithium ion secondary battery electrolyte, comprising the following components:

[0006] Non-aqueous solvents;

[0007] lithium salts; and

[0008] An additive, comprising a compound represented by any one of formula (I) to formula (III):

[0009]

[0010] Among them, R1, R2, R3 and R4 are substituents with 1-3 carbon atoms, 0-3 heteroatoms and 0-4 unsaturation degrees; R5, R6 and R7 are substituents with 1-3 carbon atoms, 0-3 heteroatoms and 0-4 unsaturation degrees; R8 is a cyclic substituent with 0-4 unsaturation degrees and 0-5 heteroatoms. When the unsaturation degree of R8 is 0, R9 is vinyl, propenyl, butenyl, 1,3-butadienyl, ethynyl, propynyl. When the unsaturation degree of R8 is 1-4, the R9 substituent does not exist; the heteroatom is selected from at least one of nitrogen, fluorine and oxygen, and n is 0-2.

[0011] In one embodiment of the present invention, R1, R2, R3 and R4 are alkyl, alkenyl, alkynyl, carbonyl, ester or amino respectively; R5, R6 and R7 are alkyl, alkenyl, alkynyl or amino respectively. In one embodiment of the present invention, the content of the additive in the electrolyte is 0.05wt%-3wt%. In one embodiment of the present invention, the content of the additive in the electrolyte is 0.1wt%-0.5wt%. In one embodiment of the present invention, the additive is selected from at least one of the following compounds: Compound 1, Compound 2, Compound 3, Compound 4 or Compound 5. In one embodiment of the present invention, the non-aqueous solvent is selected from at least one of carbonate, carboxylic acid ester, ether or nitrile, the carbonate is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate or fluoroethylene carbonate, the carboxylic acid ester is selected from at least one of ethyl formate, ethyl acetate, propyl acetate or ethyl propionate, the ether is selected from at least one of ethylene glycol dimethyl ether or diethanol diethyl ether, the nitrile is selected from at least one of acetonitrile, propionitrile, butyronitrile or valeronitrile, and the content of the non-aqueous solvent in the electrolyte is 70wt%-85wt%. In one embodiment of the present invention, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(trifluoromethyl)sulfonyl imide, lithium bis(trifluoromethyl)sulfonyl imide, lithium acetate, lithium methane sulfonate and lithium trifluoromethyl sulfonate, and the content of the lithium salt in the electrolyte is 12wt%-16wt%. The present invention also provides a lithium ion secondary battery, comprising at least: a positive electrode sheet; a negative electrode sheet; and

[0012] An electrolyte, wherein the electrolyte is selected from the lithium ion secondary battery electrolyte according to any one of claims 1 to 7.

[0013] In one embodiment of the present invention, the positive electrode active material on the positive electrode sheet includes Li x [Ni y Co z Mn tM (1-y-z-t) O 2-δ ), where M is at least one of Cr, Zr, Ca, Mg, Cu, Ti, Al, Mo, W or Zn, 0.9 < x < 1.1, 0.65 ≤ y < 1.0, 0 ≤ z < 0.5, 0 ≤ t < 0.5, 0 ≤ δ ≤ 0.1; the negative electrode active material on the negative electrode sheet includes at least one of graphite, silicon oxide material or silicon carbide material.

[0014] The present invention also provides an electrochemical device, including the lithium ion secondary battery described above.

[0015] In summary, the present invention provides a lithium ion secondary battery electrolyte and its application, which can introduce unsaturated functional groups with good lithium ion conduction ability on the positive electrode side. After adsorption, the lone pair electrons of nitrogen atoms can complex with the empty D orbitals of transition metal ions, so as to capture the transition metal ions that may escape, prevent the dissolution of transition metal ions on the positive electrode side, and prevent the internal short circuit caused by the diffusion of transition metal ions to the negative electrode and reduction, thereby improving the safety performance of the battery. At the same time, it can also improve the initial kinetics and avoid the collapse of the positive electrode caused by the overflow of transition metal ions. It can neutralize H + generated in the system, reduce the content of HF, improve the gas generation problem of the lithium ion secondary battery, improve the performance of the lithium ion secondary battery, and improve the use safety of the lithium ion secondary battery. Specific Embodiments

[0016] The following specific examples illustrate the embodiments of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.

[0017] It should be understood that the present invention can be implemented in different forms and should not be construed as limited to the embodiments presented herein. On the contrary, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.

[0018] The technical solutions of the present invention will be further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts fall within the scope of protection of the present invention.

[0019] The present invention proposes a lithium-ion secondary battery, which is, for example, a primary battery or a secondary battery, and the secondary battery is, for example, a soft-pack battery, a square-shell battery or a cylindrical battery, etc. The present invention does not specifically limit the type of lithium-ion secondary battery. Here, a square-shell battery is taken as an example to illustrate the specific implementation of the present invention. In one embodiment of the present invention, the lithium-ion secondary battery includes a shell and a bare cell arranged in the shell, and the bare cell includes a positive electrode sheet, a diaphragm and a negative electrode sheet. The positive electrode sheet, the diaphragm and the negative electrode sheet are stacked in sequence to ensure that a diaphragm is provided between any positive electrode sheet and any negative electrode sheet. The bare cell is obtained by winding or laminating, and the bare cell is loaded into a battery shell. Thereafter, an electrolyte is injected into the shell once or multiple times so that the bare cell is completely immersed in the electrolyte.

[0020] The positive electrode sheet includes a positive current collector and a positive active material layer coated on at least one surface of the positive current collector. The positive current collector is, for example, a foil formed by surface treatment of nickel, titanium, aluminum, silver, stainless steel or carbon. In addition to the foil, the positive current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. The thickness of the positive current collector is, for example, 8μm-15μm. In this embodiment, the positive current collector is, for example, aluminum foil, and the thickness of the aluminum foil is, for example, 13μm.

[0021] The positive electrode material layer includes a positive electrode active material, a binder, and a conductive agent. Among them, the positive electrode active material can be selected from a nickel-cobalt-manganese ternary positive electrode active material. The positive electrode active material can be represented by the following chemical formula: Li x [Ni y Co z Mn t M (1-y-z-t) ]O 2-δ, where M is selected from one or more of Cr, Zr, Ca, Mg, Cu, Ti, Al, Mo, W, Zn, etc., 0.9 < x < 1.1, 0.65 ≤ y < 1.0, 0 ≤ z < 0.5, 0 ≤ t < 0.5, 0 ≤ δ ≤ 0.1. Among the substances shown here, the proportion of nickel content exceeds 0.9. Compared with the conventional ternary cathode active material with a nickel content lower than 0.8, it can further improve the energy density and cycle life of the lithium-ion secondary battery. The binder is, for example, selected from any one or more of polyvinylidene fluoride (PVDF), poly(ethylene oxide) (PEO), polyamide (PA), polyacrylonitrile (PAN), polyacrylate, polyvinylether, polymethyl methacrylate (PMMA), ethylene-propylene-diene terpolymer (EPDM), polyhexafluoropropylene, polymerized styrene butadiene rubber (SBR), etc. The conductive agent is, for example, selected from any one or more of super P, acetylene black, carbon nanotubes, and graphene. In the cathode material layer, the mass ratio of the cathode active material, conductive agent, and binder is, for example, (90 - 98):(1 - 5):(1 - 5).

[0022] In an embodiment of the present invention, the cathode active material is, for example, LiNi 0.9 Mn 0.05 Co 0.05 O2, the binder is, for example, selected from polyvinylidene fluoride, and the conductive agent is, for example, selected from conductive carbon black. After mixing the cathode active material, conductive agent, and binder in a mass ratio of 98:1:1, an organic solvent is added, and the mixture is stirred under a vacuum mixer until the system becomes homogeneous to obtain the cathode slurry. Among them, the organic solvent is, for example, selected from N-methylpyrrolidone (NMP). The cathode slurry is uniformly coated on the aluminum foil, then air-dried at room temperature and transferred to an oven for drying, and the cathode electrode sheet is obtained through processes such as cold pressing and slitting. In other embodiments, the cathode electrode sheet can also be obtained by any other method of forming the cathode electrode sheet.

[0023] The negative electrode plate includes, for example, a negative electrode current collector and a negative electrode material layer coated at least on one surface of the negative electrode current collector. The negative electrode current collector is selected from, for example, a copper foil current collector, a composite copper foil current collector, a carbon current collector, a foam copper current collector, or a stainless steel current collector, etc. The thickness of the negative electrode current collector is, for example, 8 μm - 15 μm. In this embodiment, the negative electrode current collector is selected as a copper foil, and the thickness of the copper foil is, for example, 13 μm.

[0024] In an embodiment of the present invention, the negative electrode material layer includes a negative electrode active material, a conductive agent, a binder, a thickening agent, etc. Among them, the negative electrode active material is a compound capable of intercalating and deintercalating lithium ions. In an embodiment of the present invention, the negative electrode active material includes, for example, graphite, silicon oxide material (SiO x , 0 < x < 2) or at least one of silicon-carbon materials. When the negative electrode active material includes a silicon oxide material or a silicon-carbon material, its mass ratio with graphite is, for example, 5:95 - 10:90. The binder is selected from, for example, any one or more of polyvinylidene fluoride, polyethylene oxide, polyamide, polypropylene, polyacrylate, polyethylene ether, polymethyl methacrylate, polyhexafluoropropylene, or styrene-butadiene rubber, etc. The thickening agent is selected as, for example, sodium carboxymethyl cellulose (CarboxymethylCellulose Sodium, CMC-Na), etc. The conductive agent is selected from, for example, any one or more of conductive carbon black, acetylene black, Ketjen black, carbon nanotubes, and graphene, etc. The mass ratio of the negative electrode active material, the conductive agent, the binder, and the thickening agent in the negative electrode material layer is, for example, (90 - 96):(1 - 2):(1 - 3):(2 - 5).

[0025] In an embodiment of the present invention, the negative electrode active material is selected from, for example, graphite and silicon-carbon materials, and the mass ratio of the silicon-carbon material and graphite is, for example, 6:94. The conductive agent is selected from, for example, conductive carbon black. The thickening agent is selected from, for example, sodium carboxymethyl cellulose. The binder is selected from, for example, styrene-butadiene rubber. In an embodiment of the present invention, the negative electrode active material, the conductive agent, the binder, and the thickening agent are mixed, for example, according to a mass ratio of 96:1:1:2, deionized water is added, and they are mixed evenly under the action of a vacuum mixer to obtain a negative electrode slurry. The negative electrode slurry is coated on the copper foil, then dried at room temperature and transferred to an oven for drying, and after processes such as cold pressing and slitting, a negative electrode plate is obtained. In other embodiments, the negative electrode plate can also be obtained by choosing any other method of forming a negative electrode plate.

[0026] The separator is, for example, a polyethylene film (Polyethylene, PE), a polypropylene film (Polypropylene, PP), a glass fiber film, or a composite film, etc. And the thickness of the separator is, for example, 9 μm - 15 μm.

[0027] Lithium-ion secondary batteries also include an electrolyte that is injected and fills the entire internal space of the battery. The positive electrode, separator and negative electrode are completely immersed in the electrolyte. The electrolyte plays the role of conducting ions, providing ion channels and maintaining chemical stability. The various components in the electrolyte can be divided into non-aqueous solvents, lithium salts and additives according to their functions and addition amounts. Non-aqueous solvents are used to dissolve lithium salts and additives; lithium salts are mainly used to provide lithium ions to form ion channels; in the entire electrochemical system of the battery, the directional movement of lithium ions and electrons generates electricity. Lithium salts have a great influence on the energy density, power density, wide electrochemical window, cycle life and safety performance of lithium batteries. Additives are substances added in small amounts to the electrolyte. There are many types and each plays a different role. For example, they can have different improvement effects on the high and low temperature performance, cycle performance, and film-forming performance of the battery.

[0028] The present invention provides a lithium ion secondary battery electrolyte, which comprises at least a non-aqueous solvent, a lithium salt and an additive, wherein the additive comprises a compound represented by any one of formula (I) to formula (III):

[0029]

[0030] Wherein, R1, R2, R3 and R4 are substituents with 1-3 carbon atoms, 0-4 unsaturation and 0-3 heteroatoms. In one embodiment of the present invention, R1, R2, R3 and R4 are substituents such as alkyl, alkenyl, alkynyl, carbonyl, ester or amino. R5, R6 and R7 are substituents with 1-3 carbon atoms, 0-4 unsaturation and 0-3 heteroatoms. In one embodiment of the present invention, R5, R6 and R7 are substituents such as alkyl, alkenyl, alkynyl or amino. R8 is a cyclic substituent with 0-4 unsaturation and 0-5 heteroatoms. When the unsaturation of R8 is 0, R9 is vinyl, propenyl, butenyl, 1,3-butadienyl, ethynyl, propynyl, etc. When the unsaturation of R8 is 1-4, the R9 substituent does not exist. The heteroatoms included in formula (I) to formula (III) are selected from at least one of nitrogen, fluorine or oxygen, and n in formula (I) to formula (II) is 0-2. In the fully charged state, the positive electrode transition metal ion activity is high, and the positive electrode structure is + After the attack, collapse occurs and transition metal ions are easily dissolved from the positive electrode. The additives include unsaturated bonds and nitrogen atoms, which can complex the nickel ions in the positive electrode and neutralize the H+ in the system, thereby improving the safety of lithium-ion secondary batteries.

[0031] In one embodiment of the present invention, the additive is selected from Compound 1,

[0032] Compound 2, Compound 3, Compound 4 or At least one of compound 5, etc. In one embodiment of the present invention, the molecular weight of the additive is, for example, less than or equal to 200. Through the additive provided by the present application, the unsaturated bonds in the additive will cause the additive to be preferentially adsorbed on the positive electrode side, and unsaturated functional groups with good lithium ion conductivity are introduced on the positive electrode side. After adsorption, the nitrogen atom's lone pair of electrons can be used to complex with the vacant D orbital of the transition metal ion to capture the transition metal ions that may escape, which can prevent the dissolution of the transition metal ions on the positive electrode side, prevent the transition metal ions from diffusing to the negative electrode and causing internal short circuits caused by reduction, improve the safety performance of the battery, and at the same time avoid the collapse of the positive electrode caused by the overflow of transition metal ions. At the same time, the nitrogen atom in the additive has a lone pair of electrons, which can neutralize the H generated by the system. + , reduce the HF content, improve the gas production problem of lithium-ion secondary batteries, and improve the performance of lithium-ion secondary batteries.

[0033] In one embodiment of the present invention, the content of the additive in the electrolyte is, for example, 0.05wt%-3wt%, and the content includes the endpoint value. When the content of the additive is low, the neutralization ability is insufficient to improve the performance of the lithium-ion secondary battery. When the content of the additive is high, the excess additive is easy to act as a nucleophilic attacking agent, and reacts with the cyclic substances in the system, such as ethylene carbonate or fluoroethylene carbonate in the non-aqueous solvent, to undergo a ring-opening polymerization reaction, causing excessive consumption of the non-aqueous solvent and deteriorating the dynamics and high-temperature performance of the battery. In one embodiment of the present invention, the content of the additive in the electrolyte is, for example, selected to be 0.1wt%-0.5wt%. Within this range, the initial power of the battery, high-temperature storage gas production, and open circuit voltage after storage can be improved at the same time. Therefore, the added content is controlled to ensure the improvement of the comprehensive performance of the lithium-ion secondary battery.

[0034] In one embodiment of the present invention, the lithium salt is selected from at least one of lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethyl)sulfonyl imide (LiFSI), lithium bis(trifluoromethyl)sulfonyl imide (LiTFSI), lithium acetate, lithium methane sulfonate and lithium trifluoromethyl sulfonate (CF3SO3Li), and the content of the lithium salt in the electrolyte is, for example, 12wt%-16wt%. In one embodiment of the present invention, the lithium salt is selected from a mixture of lithium hexafluorophosphate and lithium bis(trifluoromethyl)sulfonyl imide, and the mass ratio of lithium hexafluorophosphate to lithium bis(trifluoromethyl)sulfonyl imide is, for example, 14:1-14:4.

[0035] In one embodiment of the present invention, the non-aqueous solvent is selected from at least one of carbonate, carboxylic acid ester, ether or nitriles, wherein the carbonate is selected from at least one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) or fluoroethylene carbonate (FEC), the carboxylic acid ester is selected from at least one of ethyl formate (EF), ethyl acetate (EA), propyl acetate (PA) or ethyl propionate (EP), and the ether is selected from ethylene glycol dimethyl ether (1,2-dimethoxyethane, DME) or diethyl glycol ether (Ethylene Glycol Diethyl Ether). The non-aqueous solvent is selected from at least one of acetonitrile (AN), propionitrile (Propionitrile), butyronitrile (BN) or valeronitrile (VN). The content of the non-aqueous solvent in the electrolyte is, for example, 70wt%-85wt%. In a specific embodiment of the present invention, the non-aqueous solvent is, for example, a mixture of ethylene carbonate and ethyl methyl carbonate. In a specific embodiment of the present invention, the non-aqueous solvent is, for example, a mixture of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate. In a specific embodiment of the present invention, the non-aqueous solvent is, for example, a mixture of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate.

[0036] In one embodiment of the present invention, when preparing the electrolyte, the content of a stable gas such as nitrogen or argon in the glove box is 99.999%, the actual oxygen content in the glove box is less than or equal to 0.1ppm, and the water content is less than or equal to 0.1ppm. After the non-aqueous solvent is mixed uniformly according to the mass ratio, the fully dried lithium salt is added to the non-aqueous solvent, and an additive is added to prepare a non-aqueous electrolyte for a lithium ion secondary battery. Among them, the content of the lithium salt and the additive, excluding the non-aqueous solvent, is the weight percentage calculated based on the total weight of the electrolyte.

[0037] In one embodiment of the present invention, the positive electrode sheet, the separator, and the negative electrode sheet are placed in sequence, so that the separator is located between the positive electrode sheet and the negative electrode sheet to play an isolating role, and a bare cell is obtained by winding or laminating. The bare cell is placed in a shell, dried in a vacuum oven, and sealed after injecting the electrolyte prepared in the present application, and at least undergoes the processes of standing, forming, and volume separation to obtain a lithium-ion secondary battery.

[0038] Hereinafter, the present invention will be explained in more detail by citing examples, which should not be construed as limiting. Appropriate modifications may be made within the scope consistent with the gist of the present invention, all of which fall within the technical scope of the present invention.

[0039] Example 1

[0040] Preparation of electrolyte: In an argon glove box with a moisture content of less than 0.1 ppm and an oxygen content of less than 0.1 ppm, ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate are mixed uniformly in a mass ratio of 3:5:2 to obtain a mixed solvent, and then dry lithium hexafluorophosphate and compound 1 are added to the mixed solvent, and the electrolyte is obtained after mixing uniformly. In the obtained electrolyte, the content of lithium salt is 12wt%, and the content of compound 1 is 0.05wt%.

[0041] Preparation of positive electrode: LiNi 0.9 Mn 0.05 Co 0.05 After mixing O2, polyvinylidene fluoride, and conductive carbon black in a mass ratio of 98:1:1, N-methylpyrrolidone is added and stirred in a vacuum mixer until the system is uniform to obtain a positive electrode slurry. The positive electrode slurry is evenly coated on aluminum foil, then dried at room temperature and transferred to an oven for drying, and the positive electrode sheet is obtained through cold pressing and slitting.

[0042] Preparation of negative electrode sheet: negative electrode active material, conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber are mixed in a mass ratio of 96:1:1:2. The negative electrode active material is a mixture of silicon-carbon material and graphite. The mass ratio of silicon-carbon material to graphite is 6:94. Deionized water is added and mixed evenly under the action of a vacuum mixer to obtain negative electrode slurry. The negative electrode slurry is coated on copper foil, and then transferred to an oven for drying after drying at room temperature. After cold pressing and slitting, the negative electrode sheet is obtained.

[0043] Selection of diaphragm: A 12 μm polyethylene film was selected as the diaphragm.

[0044] Preparation of battery: stack the positive electrode sheet, separator and negative electrode sheet in sequence, so that the separator is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, and stack the sheets to obtain a bare battery cell. Then put it into a shell, dry it in a vacuum oven, inject the above-prepared electrolyte, seal it, and perform electrolyte formation to obtain a lithium-ion secondary battery (hereinafter referred to as a battery).

[0045] Example 2

[0046] The additive was changed to compound 2, and the other steps were consistent with Example 1.

[0047] Example 3

[0048] The additive was changed to compound 4, and the content of compound 4 was 3 wt %. The other steps were the same as those in Example 1.

[0049] Example 4

[0050] The additive was changed to compound 2, and the content of compound 2 was 3 wt %. The other steps were the same as those in Example 1.

[0051] Example 5

[0052] The additive was changed to compound 2, and the content of compound 2 was 0.1 wt %. The other steps were the same as those in Example 1.

[0053] Example 6

[0054] The additive was changed to compound 2, and the content of compound 2 was 0.3 wt %. The other steps were the same as those in Example 1.

[0055] Example 7

[0056] The additive was changed to compound 2, and the content of compound 2 was 0.5 wt %. The other steps were the same as those in Example 1.

[0057] Example 8

[0058] The additive was changed to compound 2, and the content of compound 2 was 1 wt %. Other operations were consistent with Example 1.

[0059] Comparative Example 1

[0060] No additives were added, and other steps were the same as in Example 1.

[0061] Comparative Example 2

[0062] The additive was changed to compound 2, and the content of compound 2 was 5 wt %. The other steps were the same as those in Example 1.

[0063] Comparative Example 3

[0064] Additives to Compound 6, and the content of compound 6 is 0.3wt%, and other operations are consistent with Example 1.

[0065] Comparative Example 4

[0066] Additives to Compound 7, and the content of compound 7 is 0.3wt%, and other operations are consistent with Example 1.

[0067] In the present invention, lithium ion secondary batteries were prepared respectively using different electrolyte ratios as in Examples 1-8 and Comparative Examples 1-4, and the performance of each lithium ion secondary battery was tested as follows.

[0068] BOL DC resistance (DCR) test

[0069] The specific test method for testing the direct current resistance (DCR) at the beginning of life (BOL) state is as follows: adjust the temperature of the thermostat to 25°C and place the battery in the thermostat for 10 minutes; charge to 4.25V at a constant current of 0.33C, then charge to 0.05C at a constant voltage at 4.25V, let it stand for 30 minutes, then discharge to 2.5V at a constant current of 0.33C, let it stand for 10 minutes; repeat the above charge and discharge cycle twice, and take the last discharge capacity as C0. Then charge to 4.25V at a constant current of 0.33C, then charge to 0.05C at a constant voltage, let it stand for 30 minutes, then discharge to 50% C0 at a constant current of 0.33C, let it stand for 1 hour, and record the static terminal voltage at this time as V0. Finally, discharge the battery discharged to 50% C0 at a constant current of 4C0 for 30 seconds, and record the voltage at this time as V1. Then BOL DCR = (V0-V1) / 4C0.

[0070] 60℃ storage gas production test and open circuit voltage test

[0071] The specific steps of the 60℃ storage gas production test are as follows: After adjusting the temperature of the thermostat to 25℃, place the battery in the thermostat and let it stand for 2h. Charge to 4.25V at a constant current of 0.33C, then charge to 0.05C at a constant voltage, let it stand for 30min, measure the volume of the battery at this time and record it as V1, that is, V1 is the volume of the battery in the fully charged state before the battery is stored. The same battery that obtained V1 is discharged to 2.5V at a constant current of 0.33C, then adjust the temperature of the thermostat to 60℃, let it stand for 30min, charge to 4.25V at a constant current of 0.33C, then charge to 0.05C at a constant voltage, and after storing for 2 months (represented as 2M in Table 1 below), measure the battery volume and record it as V2, then the gas production volume expansion rate after 2 months of storage can be calculated = (V2-V1) / V1×100%. While measuring the battery volume, the voltage across the positive and negative electrodes of the battery is measured and recorded as the open circuit voltage (OCV), thereby obtaining the open circuit voltage after storage at 60° C. for 2 months.

[0072] Table 1. Performance test results of lithium ion secondary batteries in Examples 1-8 and Comparative Examples 1-4

[0073]

[0074] As shown in Table 1, by comparing Examples 1-8 with Comparative Example 1, it can be seen that by adding the additive provided by the present invention to the electrolyte, the initial kinetics of the lithium-ion secondary battery can be improved, and the gas generation during high-temperature storage and the open circuit voltage after storage are significantly improved. By comparing Examples 1-4, it can be seen that by selecting different compounds that conform to the general formula of the present invention as additives, the performance of the lithium-ion secondary battery is improved. This is presumably because: by adding compounds that contain both unsaturated bonds and nitrogen atoms and conform to the general formula of the present invention to the electrolyte, they can all complex the transition metal ions of the positive electrode and neutralize the system to produce H + , improving the battery's initial power, high-temperature storage gas production and open-circuit voltage after storage, but additives with different structures have different effects on improving performance. As shown in Table 1, compound 2 has the most obvious effect on the improvement of the battery's initial kinetics, high-temperature storage gas production and open-circuit voltage after storage.

[0075] Please refer to Table 1, comparing Examples 2, 5-8 and Comparative Example 2, when the content of the specific compound shown in the additive is in the range of 0.05wt%-3wt%, the initial dynamics and high-temperature storage performance of the battery are improved, and as the content of the additive increases, the DCR of the lithium-ion secondary battery first decreases and then increases, the high-temperature storage gas production first decreases and then increases, and the high-temperature storage OCV first increases and then decreases. Therefore, controlling the content of the additive can optimize the comprehensive performance of the lithium-ion secondary battery. When the content of the additive exceeds 3wt%, a thicker SEI film will be formed at the negative electrode, resulting in deterioration of the performance of the lithium-ion secondary battery.

[0076] Furthermore, by comparing Examples 1-8 with Comparative Examples 3-4, it can be seen that when the compound in the additive contains only unsaturated bonds or only nitrogen atoms, the performance of the lithium-ion secondary battery is not significantly improved, indicating that only when the additive contains a compound with a specific structure of unsaturated bonds and nitrogen atoms at the same time can the battery's initial power, high-temperature storage gas production, and open circuit voltage after storage be improved.

[0077] The present invention also provides an electronic device, the electronic device includes at least one of the above-mentioned lithium ion secondary batteries, and the lithium ion secondary battery is used to provide electrical energy. Among them, the electronic device can be a vehicle, a mobile phone, a portable device, a laptop computer, a ship, a spacecraft, an electric toy and an electric tool, etc. In one embodiment of the present invention, the vehicle is, for example, a new energy vehicle, and the new energy vehicle can be a pure electric vehicle, a hybrid vehicle or an extended-range vehicle, etc. Spacecraft include airplanes, rockets, space shuttles and spacecrafts, etc., and electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys and electric airplane toys, etc. Electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers, etc. The electronic device includes the above-mentioned lithium ion secondary battery, so the advantages of the above-mentioned lithium ion secondary battery are included, which will not be elaborated here.

[0078] In summary, the present invention proposes a lithium ion secondary battery electrolyte and its application. By adding a compound with a specific structure containing both unsaturated bonds and nitrogen atoms to the electrolyte, an unsaturated functional group with good lithium ion conductivity can be introduced on the positive electrode side. After adsorption, the lone pair of electrons of the nitrogen atom can be used to complex with the vacant D orbital of the transition metal ion to capture the transition metal ions that may escape, and the dissolution of the transition metal ions on the positive electrode side can be prevented, and the internal short circuit caused by the diffusion of the transition metal ions to the negative electrode for reduction can be prevented, thereby improving the safety performance of the battery. At the same time, it can also improve the initial kinetics and avoid the collapse of the positive electrode caused by the overflow of the transition metal ions. It can neutralize the H generated by the system. +, reduce the HF content, improve the gas production problem of lithium-ion secondary batteries, improve the performance of lithium-ion secondary batteries, and improve the safety of lithium-ion secondary batteries.

[0079] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0080] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A lithium ion secondary battery electrolyte, characterized in that: At least the following components are included: Non-aqueous solvents; Lithium salts; as well as An additive, comprising a compound represented by any one of formula (I) to formula (III): Among them, R1, R2, R3 and R4 are substituents with 1-3 carbon atoms, 0-3 heteroatoms and 0-4 unsaturation degrees; R5, R6 and R7 are substituents with 1-3 carbon atoms, 0-3 heteroatoms and 0-4 unsaturation degrees; R8 is a cyclic substituent with 0-4 unsaturation degrees and 0-5 heteroatoms. When the unsaturation degree of R8 is 0, R9 is vinyl, propenyl, butenyl, 1,3-butadienyl, ethynyl, propynyl. When the unsaturation degree of R8 is 1-4, the R9 substituent does not exist; the heteroatom is selected from at least one of nitrogen, fluorine and oxygen, and n is 0-2.

2. The lithium ion secondary battery electrolyte according to claim 1, characterized in that: R1, R2, R3 and R4 are respectively alkyl, alkenyl, alkynyl, carbonyl, ester or amino; R5, R6 and R7 are respectively alkyl, alkenyl, alkynyl or amino.

3. The lithium ion secondary battery electrolyte according to claim 1, characterized in that: The content of the additive in the electrolyte is 0.05wt%-3wt%.

4. The lithium ion secondary battery electrolyte according to claim 3, characterized in that: The content of the additive in the electrolyte is 0.1wt%-0.5wt%.

5. The lithium ion secondary battery electrolyte according to claim 1, characterized in that: The additive is selected from at least one of the following compounds:

6. The lithium ion secondary battery electrolyte according to claim 1, characterized in that: The non-aqueous solvent is selected from at least one of carbonates, carboxylates, ethers or nitriles, the carbonate is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate or fluoroethylene carbonate, the carboxylate is selected from at least one of ethyl formate, ethyl acetate, propyl acetate or ethyl propionate, the ether is selected from at least one of ethylene glycol dimethyl ether or diethanol diethyl ether, the nitrile is selected from at least one of acetonitrile, propionitrile, butyronitrile or valeronitrile, and the content of the non-aqueous solvent in the electrolyte is 70wt%-85wt%.

7. The lithium ion secondary battery electrolyte according to claim 1, characterized in that: The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethyl)sulfonylimide, lithium acetate, lithium methanesulfonate and lithium trifluoromethylsulfonate, and the content of the lithium salt in the electrolyte is 12wt%-16wt%.

8. A lithium ion secondary battery, characterized in that: At least: Positive electrode; Negative electrode; as well as An electrolyte, wherein the electrolyte is selected from the lithium ion secondary battery electrolyte according to any one of claims 1 to 7.

9. The lithium ion secondary battery according to claim 8, characterized in that: The positive active material on the positive electrode plate includes Li x [Ni y Co z Mn t M (1-y-z-t) O 2-δ , where M is at least one of Cr, Zr, Ca, Mg, Cu, Ti, Al, Mo, W or Zn, 0.9 < x < 1.1, 0.65 ≤ y < 1.0, 0 ≤ z < 0.5, 0 ≤ t < 0.5, 0 ≤ δ ≤ 0.1; the negative active material on the negative electrode plate includes at least one of graphite, silicon oxide material or silicon carbide material.

10. An electrochemical device, characterized in that: A lithium ion secondary battery comprising any one of claims 8 to 9.