Method for manufacturing capacitor for dram and electronic device

By using a capping layer to provide stress during the dielectric layer annealing process, the lateral grain growth of the dielectric layer material is promoted, thus solving the problems of high dielectric constant and low leakage current in DRAM capacitors and manufacturing high-performance capacitors.

CN118785698APending Publication Date: 2024-10-15BEIJING SUPERSTRING ACAD OF MEMORY TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310352954.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously achieve high dielectric constant and low leakage current in DRAM capacitors, especially when the dielectric layer thickness is less than 10 nm.

Method used

By using a capping layer to provide stress during the annealing process of the dielectric layer, longitudinal crystallization is suppressed, lateral grain growth of the dielectric layer material is promoted, and crystallization quality is improved. High-performance capacitors can be manufactured using specific materials and annealing conditions.

Benefits of technology

High-performance capacitors with dielectric constants greater than 100 and leakage current less than 10⁻⁷ A/cm² were manufactured, significantly improving the storage capacity of capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118785698A_ABST
    Figure CN118785698A_ABST
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a capacitor for a DRAM (Dynamic Random Access Memory) and electronic equipment. The method comprises the following steps: depositing a first conductive layer on a substrate; depositing a dielectric substance layer on one side, far away from the substrate, of the first conductive layer; depositing a covering layer on one side, far away from the substrate, of the dielectric substance layer; annealing is carried out on the first conductive layer, the dielectric substance layer and the covering layer; etching to remove the covering layer; and depositing a second conductive layer on one side, far away from the substrate, of the annealed dielectric substance layer. The first conductive layer, the dielectric substance layer and the covering layer are annealed, the stress effect provided by the covering layer for the dielectric substance layer during annealing is utilized, longitudinal crystallization of an amorphous dielectric substance layer material during annealing crystallization is inhibited, transverse crystallization of crystal grains of the dielectric substance layer material is effectively promoted, the crystallization quality of the dielectric substance layer material is improved, and the performance of the device is improved. Dielectric constant value is increased, electric leakage path is reduced, electric leakage is reduced, and storage capacity of the capacitor is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to, but is not limited to, the field of capacitor structure preparation, and in particular to a method for manufacturing a capacitor for DRAM and an electronic device. Background Art

[0002] As dynamic random access memory (DRAM) continues to shrink, the capacitor of DRAM is challenged: it needs to meet the requirements of high dielectric constant and low leakage at the same time. The ideal dielectric layer material has high dielectric constant (k>100), low leakage (<10e -7 A / cm 2 ), and its physical thickness must be less than 10nm. Summary of the invention

[0003] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.

[0004] The present application provides a method for manufacturing a capacitor and an electronic device. The method of the present application improves the crystal quality of dielectric layer materials, increases the k value, reduces leakage paths, and reduces leakage.

[0005] The present application provides a method for manufacturing a capacitor for a DRAM, comprising:

[0006] depositing a first conductive layer on the substrate;

[0007] Depositing a dielectric layer on a side of the first conductive layer away from the substrate;

[0008] depositing a capping layer on a side of the dielectric layer away from the substrate;

[0009] annealing the first conductive layer, the dielectric layer and the capping layer;

[0010] Etching to remove the covering layer;

[0011] depositing a second conductive layer on a side of the annealed dielectric layer away from the substrate;

[0012] The cover layer is configured to enable the crystal grains in the dielectric layer to grow laterally in a direction parallel to the substrate during annealing.

[0013] In an embodiment of the present application, the material of the covering layer is selected from Group IVB metals and their nitrides or oxides; or selected from Group VB metals and their nitrides or oxides; or selected from Group VIB metals and their nitrides or oxides; or selected from Si and its nitrides, oxides or oxynitrides; or selected from Ge and its nitrides, oxides or oxynitrides.

[0014] In an embodiment of the present application, the material of the cover layer is selected from any one or more of titanium nitride, tantalum nitride, chromium, tungsten, silicon, silicon dioxide, silicon oxynitride and silicon nitride.

[0015] In an embodiment of the present application, the thickness of the covering layer is 10-50 nm.

[0016] In the embodiments of the present application, the annealing temperature is 500-600° C., the annealing time is 30s-120s, and the annealing atmosphere is a vacuum, nitrogen or argon environment.

[0017] In the embodiment of the present application, the annealing temperature is 550-600° C., and the annealing time is 60s-120s.

[0018] In an embodiment of the present application, the material of the dielectric layer includes a main material and a doping material, and the main material is a strontium titanate material.

[0019] In an embodiment of the present application, the doping material is selected from any one or more of Si, Hf, Y, Al, Zr and Gd.

[0020] In an embodiment of the present application, a material of the first conductive layer or the second conductive layer is metal, alloy, or metal oxide.

[0021] The present application embodiment provides a capacitor manufactured by the above method, comprising:

[0022] a first conductive layer disposed on the substrate;

[0023] a dielectric layer located on a side of the first conductive layer away from the substrate; and

[0024] A second conductive layer is located on a side of the dielectric layer away from the substrate.

[0025] In an embodiment of the present application, cross-sections of the first conductive layer, the dielectric layer, and the second conductive layer are annular.

[0026] An embodiment of the present application also provides an electronic device, comprising the above-mentioned capacitor.

[0027] The method for manufacturing a capacitor in the embodiment of the present application anneals the first conductive layer, the dielectric layer and the cover layer, and utilizes the stress provided by the cover layer to the dielectric layer during annealing to inhibit the longitudinal crystallization of the amorphous dielectric layer material during annealing crystallization, effectively promote the lateral crystallization of the grains of the dielectric layer material, improve the crystallization quality of the dielectric layer material, increase the k value, reduce the leakage path, reduce the leakage, and thus significantly improve the storage capacity of the capacitor. The method provided in the embodiment of the present application can manufacture a dielectric layer with a thickness of less than 10nm, a dielectric constant greater than 100, and a leakage of less than 10 -7 A / cm 2 High performance capacitors.

[0028] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by implementing the present application. Other advantages of the present application can be realized and obtained by the schemes described in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings are used to provide an understanding of the technical solution of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present application and do not constitute a limitation on the technical solution of the present application.

[0030] Figure 1 A flowchart of a method for manufacturing a capacitor according to an embodiment of the present application;

[0031] Figure 2 A schematic longitudinal cross-sectional structure diagram of an intermediate product obtained in an intermediate step of a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application in the a-a' direction;

[0032] Figure 3 A schematic diagram of the longitudinal cross-sectional structure of an intermediate product obtained in an intermediate step of a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application in the a-a' direction;

[0033] Figure 4 A schematic diagram of the longitudinal cross-sectional structure of an intermediate product obtained in an intermediate step of a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application in the a-a' direction;

[0034] Figure 5 A schematic longitudinal cross-sectional structure diagram of an intermediate product obtained in an intermediate step of a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application in the a-a' direction;

[0035] Figure 6 A schematic longitudinal cross-sectional structure diagram of an intermediate product obtained in an intermediate step of a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application in the a-a' direction;

[0036] Figure 7 FIG. 1 is a schematic diagram of a longitudinal cross-sectional structure of a capacitor in the aa′ direction obtained by a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application.

[0037] 1-substrate; 2-first conductive layer; 3-dielectric layer; 4-covering layer; 5-second conductive layer. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present application more clear, the embodiments of the present application will be described in detail below with reference to the accompanying drawings. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.

[0039] The embodiments herein can be implemented in a plurality of different forms. A person skilled in the art can easily understand the fact that the implementation and content can be transformed into various forms without departing from the purpose and scope of the present application. Therefore, the present application should not be interpreted as being limited to the contents recorded in the following embodiments. In the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined arbitrarily with each other.

[0040] The proportions of the drawings in this application can be used as a reference in the actual process, but are not limited to this. For example, the aspect ratio of the semiconductor layer, the thickness and spacing of each film layer can be adjusted according to actual needs. The drawings described in this application are only schematic diagrams of the structure, and one embodiment of this application is not limited to the shapes or values ​​shown in the drawings.

[0041] In this specification, for the sake of convenience, the words and phrases indicating the orientation or positional relationship such as "middle", "upper", "lower", "front", "back", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like are used to illustrate the positional relationship of the constituent elements with reference to the drawings. This is only for the convenience of describing this specification and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation on this application. The positional relationship of the constituent elements is appropriately changed according to the direction in which each constituent element is described. Therefore, it is not limited to the words and phrases described in the specification and can be appropriately replaced according to the situation.

[0042] In this specification, unless otherwise clearly specified and limited, the terms "disposed" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate, or the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0043] In the present disclosure, “parallel” means approximately parallel or almost parallel, for example, a state where the angle formed by two straight lines is greater than -10° and less than 10°, and therefore, a state where the angle is greater than -5° and less than 5° is also included.

[0044] In the present disclosure, "film" and "layer" may be interchanged. For example, "conductive layer" may be replaced with "conductive film" in some cases. Similarly, "dielectric film" may be replaced with "dielectric layer" in some cases.

[0045] In the description of the present application, ordinal numbers such as "first" and "second" are provided to avoid confusion among constituent elements rather than to limit the quantity.

[0046] The present application provides a method for manufacturing a capacitor, the method comprising:

[0047] depositing a first conductive layer on the substrate;

[0048] Depositing a dielectric layer on a side of the first conductive layer away from the substrate;

[0049] depositing a capping layer on a side of the dielectric layer away from the substrate;

[0050] annealing the first conductive layer, the dielectric layer and the capping layer;

[0051] Etching to remove the covering layer;

[0052] depositing a second conductive layer on a side of the annealed dielectric layer away from the substrate,

[0053] The cover layer is configured to enable the crystal grains in the dielectric layer to grow laterally in a direction parallel to the substrate during annealing.

[0054] The method for manufacturing a capacitor in the embodiment of the present application performs rapid thermal annealing on the first conductive layer, the dielectric layer and the covering layer, and utilizes the stress provided by the covering layer to the dielectric layer during annealing to inhibit the longitudinal crystallization of the amorphous dielectric layer material during annealing crystallization, effectively promoting the lateral crystallization of the grains of the dielectric layer material in a direction parallel to the substrate, thereby improving the crystallization quality of the dielectric layer material, increasing the k value, reducing the leakage path, and reducing the leakage, thereby significantly improving the storage capacity of the capacitor. The method provided in the embodiment of the present application can manufacture a dielectric layer with a thickness of less than 10nm, a dielectric constant greater than 100, and a leakage of less than 10 -7 A / cm 2 High performance capacitors.

[0055] Figure 1 The present invention is a flowchart of a method for manufacturing a capacitor according to an embodiment of the present invention.

[0056] like Figure 1 As shown, in an exemplary embodiment of the present application, a method for manufacturing a capacitor includes the following steps:

[0057] depositing a first conductive layer on the substrate;

[0058] Depositing a dielectric layer on a side of the first conductive layer away from the substrate;

[0059] depositing a capping layer on a side of the dielectric layer away from the substrate;

[0060] annealing the first conductive layer, the dielectric layer and the capping layer;

[0061] Etching to remove the covering layer;

[0062] depositing a second conductive layer on a side of the annealed dielectric layer away from the substrate,

[0063] The cover layer is configured to enable the crystal grains in the dielectric layer to grow laterally in a direction parallel to the substrate during annealing.

[0064] In an embodiment of the present application, the material of the covering layer is selected from Group IVB metals and their nitrides or oxides; or selected from Group VB metals and their nitrides or oxides; or selected from Group VIB metals and their nitrides or oxides; or selected from Si and its nitrides, oxides or oxynitrides; or selected from Ge and its nitrides, oxides or oxynitrides.

[0065] In an embodiment of the present application, the material of the cover layer is selected from any one or more of titanium nitride, tantalum nitride, chromium, tungsten, silicon, silicon dioxide, silicon oxynitride and silicon nitride.

[0066] In an embodiment of the present application, the thickness of the covering layer is 10-50 nm.

[0067] In the embodiments of the present application, the annealing temperature is 500-600° C., the annealing time is 30s-120s, and the annealing atmosphere is a vacuum, nitrogen or argon environment.

[0068] In the embodiment of the present application, the annealing temperature is 550-600° C., and the annealing time is 60s-120s.

[0069] In an embodiment of the present application, the material of the dielectric layer includes a main material and a doping material, and the main material is a strontium titanate material.

[0070] In an embodiment of the present application, the doping material is selected from any one or more of Si, Hf, Y, Al, Zr and Gd.

[0071] In an embodiment of the present application, the material of the first conductive layer or the second conductive layer is a metal, an alloy, or a metal oxide. For example, the material of the first conductive layer and the second conductive layer is independently selected from one or more of Ru, Ti, Ta, TiN and TaN.

[0072] In an embodiment of the present application, the thickness of the first conductive layer and the second conductive layer are respectively 10-20 nm, and the thickness of the dielectric layer is 5-10 nm.

[0073] In an embodiment of the present application, dry etching or wet etching is used to remove the annealed capping layer.

[0074] Figures 2 to 6 It is a schematic diagram of the longitudinal cross-sectional structure along the aa′ direction of an intermediate product obtained in an intermediate step of a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application. Figure 7 FIG. 1 is a schematic diagram of a longitudinal cross-sectional structure of a capacitor in the aa′ direction obtained by a method for manufacturing a vertically stacked capacitor according to an exemplary embodiment of the present application.

[0075] like Figures 2 to 7 As shown, in an exemplary embodiment of the present application, a method for manufacturing a capacitor may include:

[0076] S10: grow a nanowire substrate 1, deposit a first conductive layer 2 on the substrate 1, and obtain Figure 2 Intermediate products shown;

[0077] S20: Depositing a dielectric layer 3 on the first conductive layer 2 to obtain Figure 3The intermediate product shown, wherein the material of the dielectric layer is a doped strontium titanate material, the impurity atoms in the doped strontium titanate layer are one of Si, Hf, Y, Al, Zr, and Gd, and the thickness of the dielectric layer is 5-10 nm;

[0078] S30: depositing a capping layer 4 on the dielectric layer 3 to obtain Figure 4 The intermediate product shown, wherein the material of the cover layer is selected from Group IVB metals and their nitrides or oxides; or from Group VB metals and their nitrides or oxides; or from Group VIB metals and their nitrides or oxides; or from Si and its nitrides, oxides or oxynitrides; or from Ge and its nitrides, oxides or oxynitrides. For example, the material of the cover layer is selected from any one or more of titanium nitride, tantalum nitride, chromium, tungsten, silicon, silicon dioxide, silicon oxynitride and silicon nitride;

[0079] S40: annealing the first conductive layer 2, the dielectric layer 3 and the cover layer 4. Figure 5 As shown, the annealing temperature of the annealing is 500-600°C, the annealing time is 30s-120s, and the annealing atmosphere is a vacuum, nitrogen or argon environment;

[0080] S50: Etching and removing the cover layer 4 to obtain Figure 6 Intermediate products shown;

[0081] S60: depositing a second conductive layer 5 on the annealed dielectric layer 3 to obtain Figure 7 capacitor shown.

[0082] In an embodiment of the present application, the material of the covering layer is selected from Group IVB metals and their nitrides or oxides; or selected from Group VB metals and their nitrides or oxides; or selected from Group VIB metals and their nitrides or oxides; or selected from Si and its nitrides, oxides or oxynitrides; or selected from Ge and its nitrides, oxides or oxynitrides.

[0083] In an embodiment of the present application, the material of the covering layer is selected from any one or more of titanium nitride, tantalum nitride, chromium, tungsten, silicon, silicon dioxide, silicon oxynitride and silicon nitride.

[0084] In an embodiment of the present application, the material of the dielectric layer is a doped strontium titanate material.

[0085] In an embodiment of the present application, the impurity atoms in the doped strontium titanate material are any one of Si, Hf, Y, Al, Zr and Gd.

[0086] In an embodiment of the present application, the material of the first conductive layer or the second conductive layer is a metal, an alloy, or a metal oxide. For example, the material of the first conductive layer and the second conductive layer is independently selected from one or more of Ru, Ti, Ta, TiN and TaN.

[0087] In the embodiments of the present application, the substrate may be a single crystal silicon substrate, or a semiconductor on insulator (SOI) substrate, for example, a silicon on sapphire (SOS) substrate, a silicon on glass (SOG) substrate, an epitaxial layer of silicon on a base semiconductor, or other semiconductor or optoelectronic materials, such as silicon-germanium (Si 1-x Ge x , where x can be a mole fraction between 0.2 and 0.8, for example), germanium (Ge), gallium arsenide (GaAs), gallium nitride (GaN), or indium phosphide (InP). The substrate can be doped or undoped.

[0088] In an embodiment of the present application, the method of depositing the first conductive layer, the covering layer and the second conductive layer can be independently selected from any one of atomic layer deposition (ALD) and chemical vapor deposition (CVD).

[0089] In an embodiment of the present application, the method of depositing the dielectric layer may be atomic layer deposition.

[0090] The present application also provides a capacitor manufactured by the above method, including:

[0091] A first conductive layer 2 located on the substrate 1;

[0092] a dielectric layer 3 located on a side of the first conductive layer 2 away from the substrate; and

[0093] A second conductive layer 5 is located on a side of the dielectric layer 3 away from the substrate.

[0094] In the embodiment of the present application, the cross sections of the first conductive layer 2 , the dielectric layer 3 and the second conductive layer 5 are all annular.

[0095] An embodiment of the present application also provides an electronic device, comprising the capacitor provided in the above embodiment of the present application.

[0096] In an embodiment of the present application, the electronic device may include a storage device, a smart phone, a computer, a tablet computer, an artificial intelligence device, a wearable device, or a mobile power source.

[0097] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of protection of this application shall still be based on the scope defined in the attached claims.

Claims

1. A method for manufacturing a capacitor for DRAM, It is characterized in that include: depositing a first conductive layer on the substrate; Depositing a dielectric layer on a side of the first conductive layer away from the substrate; depositing a capping layer on a side of the dielectric layer away from the substrate; annealing the first conductive layer, the dielectric layer and the capping layer; Etching to remove the covering layer; depositing a second conductive layer on a side of the annealed dielectric layer away from the substrate; The cover layer is configured to enable the crystal grains in the dielectric layer to grow laterally in a direction parallel to the substrate during annealing.

2. The method according to claim 1, in, The material of the covering layer is selected from Group IVB metals and their nitrides or oxides; or, The material of the covering layer is selected from Group VB metals and their nitrides or oxides; or The material of the covering layer is selected from the group consisting of Group VIB metals and their nitrides or oxides; or The material of the cover layer is selected from Si and its nitride, oxide or oxynitride; or The material of the capping layer is selected from Ge and its nitride, oxide or oxynitride.

3. The method according to claim 1, in, The material of the cover layer is selected from any one or more of titanium nitride, tantalum nitride, chromium, tungsten, silicon, silicon dioxide, silicon oxynitride and silicon nitride.

4. The method according to claim 1, in, The thickness of the covering layer is 10-50 nm.

5. The method according to claim 1, in, The annealing temperature of the annealing is 500-600° C., the annealing time is 30s-120s, and the annealing atmosphere is a vacuum, nitrogen or argon environment.

6. The method according to claim 3, in, The annealing temperature of the annealing is 550-600° C., and the annealing time is 60s-120s.

7. The method according to claim 1, in, The material of the dielectric layer includes a main material and a doping material, and the main material is a strontium titanate material.

8. The method according to claim 5, in, The doping material is selected from any one or more of Si, Hf, Y, Al, Zr and Gd.

9. The method according to claim 1, in, The material of the first conductive layer or the second conductive layer is metal, alloy, or metal oxide.

10. An electronic device, It is characterized in that Comprising a capacitor manufactured by the method according to any one of claims 1-9.