Soldering flux and soldering method

By using a flux of rosin ester and phenyl glycol solvents, combined with an organic hydrofluoride and an auxiliary activator, the problem that the existing technology cannot wet the enameled aluminum wire is solved, and the enameled aluminum wire can be removed without peeling off the flux. High-quality welding results.

CN118786003APending Publication Date: 2024-10-15ISHIKAWA KINZOKU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092781.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-02-28
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing fluxes cannot effectively wet the enameled aluminum wire without stripping the enameled aluminum wire, resulting in poor welding quality.

Method used

Using a flux containing rosin ester and phenyl glycol solvent, combined with organic hydrofluoride and auxiliary activator, the solder wets the aluminum wire through heat and dissolves the surface oxide film to achieve welding.

Benefits of technology

Without stripping off the enameled aluminum wire, the flux can effectively wet and weld the enameled aluminum wire to ensure welding quality and is suitable for lightweight enameled aluminum wire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015291790000141
    Figure BDA0005015291790000141
  • Figure BDA0005015291790000151
    Figure BDA0005015291790000151
  • Figure HDA0005015291800000011
    Figure HDA0005015291800000011
Patent Text Reader

Abstract

There is no flux capable of soldering the enameled aluminum wire to an object to be joined without peeling off the enamel of the enameled aluminum wire. A flux which contains a rosin ester, a rosin other than the rosin ester, at least one of diethylene glycol monophenyl ether and propylene glycol monophenyl ether as a solvent, and (as an active agent) an organic hydrofluoride salt, and which is capable of wetting an enameled aluminum wire with solder without peeling off the enameled aluminum wire and soldering the enameled aluminum wire to an object to be bonded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a flux used in welding, and more particularly to a flux and a welding method capable of welding enameled aluminum wires without peeling off the enameled wires, and electric and electronic components welded using the flux. Background Art

[0002] Enameled coil wire (hereinafter also referred to as "enameled wire") is a wire that is coated with a resin such as polyurethane around the conductor so that the wires do not conduct even if they touch each other. The coating thickness is very thin, and when winding the coil, the wires will not cause a short circuit even if they touch each other. In addition, the volume does not become large when rolled up. Therefore, enameled wire can be used for coils and is also called magnet wire.

[0003] Basically, enameled wires are joined by stripping off the enameled coating on the surface and then welding in a conventional manner. The flux used at this time is a conventional flux. The flux is mainly composed of rosin composed of rosin acid, a solvent mainly composed of isopropyl alcohol as a solvent for melting the rosin, an activator, and other additives.

[0004] There are two types of enameled wires: wires with copper as the lead wire (hereinafter referred to as "enameled copper wire") and wires with aluminum as the lead wire (hereinafter referred to as "enameled aluminum wire"). Since the specific gravity of enameled aluminum wire, which has aluminum as the lead wire, is lighter than copper, even if a coil is made with a large number of windings, the weight can be made lighter. In addition, since enameled aluminum wire uses inexpensive aluminum, the product price can be reduced.

[0005] Patent Document 1 (Japanese Patent No. 6177383) discloses a method of performing welding by peeling off enamel using ultrasonic vibration.

[0006] Patent Document 2 (Japanese Patent Application Laid-Open No. 2002-059293) discloses a flux for aluminum welding, which is a mixture of 3.0 to 5.0 mass % of metal fluoride salts, 10.0 to 30.0 mass % of metal salts of organic acids, and the remainder being hydrofluoric acid salts of amino alcohols. Prior art literature Patent Literature

[0007] Patent Document 1: Japanese Patent No. 6177383 Patent Document 2: Japanese Patent Application Publication No. 2002-059293 Summary of the invention Technical problem to be solved by the invention

[0008] For enameled copper wire, the wettability of solder to copper is very high, and the solder can wet the copper wire only with molten solder and conventional flux. In other words, soldering is possible without removing the enameled wire. However, in the case of enameled aluminum wire, even if the molten solder melts the enameled wire on the surface, the solder cannot fully wet the aluminum wire. Furthermore, the enameled wire cannot be removed with flux for aluminum wire, and the solder cannot wet the enameled aluminum wire only with molten solder and conventional flux. Solutions to technical problems

[0009] The present invention has been conceived in view of the above-mentioned technical problems, and provides a flux capable of making solder wet the enameled aluminum wire even without peeling off the enameled wire.

[0010] More specifically, the soldering flux of the present invention contains rosin, specifically rosin ester, having good affinity with enamel.

[0011] Furthermore, it contains 30 to 75% by mass of a diol solvent having a phenyl group and an organic hydrofluoric acid salt, and the diol solvent having a phenyl group is specifically at least one of diethylene glycol monophenyl ether and propylene glycol monophenyl ether. Effects of the Invention

[0012] In the soldering flux of the present invention, the rosin ester and the diol solvent having a phenyl group can melt the enameled wire, and the activator can dissolve the surface oxide film of the wire. Therefore, welding can be performed only by the heat of the solder without peeling off the enameled wire. In particular, welding can be performed when the wire is an aluminum wire, and even a lightweight enameled aluminum wire (enameled aluminum wire) can be properly welded. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 The diagram shows the appearance of the object to be joined used in the experiment. Figure 2 It is a diagram explaining the experimental process. DETAILED DESCRIPTION

[0014] The soldering flux of the present invention is described below with reference to the accompanying drawings and examples. In addition, the following description is only an illustration of one embodiment and one example of the present invention, and the present invention is not limited to the following description. The following description can be changed without departing from the main purpose of the present invention. Among them, "~" means above or below. For example, "A~B" means a range including A values ​​that are greater than A (above A) and B values ​​that are smaller than B (below B).

[0015] <Rosin> The soldering flux of the present invention is composed of rosin, a solvent and an activator. Rosin can be used in combination with rosin ester and rosin other than rosin ester. Rosin ester is rosin having a hydroxyl value. Whether the soldering flux contains rosin ester can be detected by FT-IR (Infrared Spectroscopy) or GPC (Gel Permeation Chromatography).

[0016] The content of rosin is 20% to 55% by mass relative to the total amount of flux. Among them, the content of rosin ester is preferably 5% to 45% by mass relative to the total amount of flux. If the rosin ester is too little, the enameled aluminum wire (enameled aluminum wire) cannot be wetted. If the rosin ester is too much, the viscosity is too high and it cannot be used as a flux.

[0017] As rosin other than rosin ester, rosin composed of rosin acid, hydrogenated rosin, polymerized rosin, acrylic acid-modified rosin, etc. are preferably used. In addition, the content of rosin other than rosin ester is preferably 10% by mass or more relative to the total amount of the flux.

[0018] <Solvent> The solvent may be a good solvent for the resin having a boiling point lower than 400°C. Here, 400°C is the normal soldering operation temperature of lead-free solder. In addition, the boiling point of the solvent is preferably above 220°C. 220°C is the melting point of lead-free solder. This is because if the solvent evaporates before the lead-free solder melts, the effect of the solder wetting the wire is reduced. That is, if it is a good solvent for the resin having a boiling point higher than the melting point of the lead-free solder and lower than the operating temperature, it can be used as a solvent for the flux of the present invention.

[0019] Specifically, a phenyl group-containing glycol solvent is preferred, more specifically diethylene glycol monophenyl ether and propylene glycol monophenyl ether.

[0020] As an auxiliary to the enamel removal function, a good solvent for enamel, such as N-methyl-2-pyrrolidone, 3-methylphenol, chloroform, hexafluoro-2-propanol, 2-chlorophenol, etc., may be added.

[0021] The solvent may be present in an amount of 25 to 75% by mass relative to the total amount of the flux. If the amount is less than this, the rosin may not be sufficiently melted, and the flux may crystallize during storage or operation.

[0022] <Activator> The activator dissolves the enamel and removes the metal oxide film from the exposed surface of the wire, thereby making the solder easier to wet. In particular, when the wire is aluminum, an activator that can remove a strong oxide film and only works at high temperatures during soldering and does not work at room temperature is preferred. Among them, hydrofluoric acid salts of organic amines are suitable.

[0023] Specifically, hydrofluoric acid salts of amines are preferred. Specifically, hydrofluoric acid salts of cyclohexylamine, 1,3-diphenylguanidine, N,N'-diethylaniline, diethylamine, and the like can be used.

[0024] When amine hydrochloride or hydrobromide is used instead of amine hydrofluoride, the oxide film removal capability is weak, and the oxide film removal and welding on the aluminum surface by the activator cannot be completed.

[0025] Furthermore, when using an inorganic acid, hydrofluoric acid, or a salt other than an amine, sodium fluoride, the oxide film removal capability is demonstrated not only at the high temperature during welding but also at room temperature after welding, and corrosion and subsequent destruction occur at the welded portion.

[0026] Amine hydrofluoric acid salts can be used alone or in combination. The amount of the activator added is 1.2 to 5.0% by mass relative to the total amount of the flux. If it is less than 1.2% by mass, the weldability will be poor, and if it exceeds the above amount, a large amount of fluorine will remain in the flux residue, which may cause corrosion at the welding site and reduce electrical reliability.

[0027] <Assisted active agent> In addition, in the flux of the present invention, it is also suitable to use an organic bromide that generates hydrobromic acid at the welding temperature as an auxiliary activator, such as 2,3-dibromo-1-propanol, 1,2,5,6,9,10-hexabromocyclododecane, tris(2,3-dibromopropyl)isocyanurate, 2,2-bis(4-bromomethyl)-1,3-propanediol, etc.

[0028] These auxiliary activators continue to exhibit a mild oxide removal effect even after the oxide film on the surface of the aluminum wire is removed by the amine fluoride, and prevent the reoxidation of aluminum, thereby ensuring good weldability.

[0029] The amount of the auxiliary activator is preferably 0.5 to 5% by mass relative to the total amount of the flux. If the amount is less than the above, the oxide removal effect cannot be obtained, and if the amount is more than the above, a large amount of halogen will remain in the flux residue, which may cause problems in terms of corrosion and electrical reliability.

[0030] The following is a description of a soldering method using the soldering flux of the present invention. The soldering flux of the present invention contains rosin and thus has a moderate viscosity. Therefore, soldering can be performed by immersing the contact portion in the soldering flux while the enameled wire is in contact with the object to be joined, and then immersing the contact portion in the soldering flux so that the soldering flux adheres, and then immersing the contact portion in molten solder. After these steps, a step of cleaning the joined object after soldering can be performed.

[0031] In order to adjust the viscosity and thixotropy of the flux for the purpose of controlling the amount of the flux attached to the contact portion, wax, gelling agent, etc. may be added as in conventional liquid flux or paste flux.

[0032] Here, the object to be bonded is a conductive metal. It is usually copper, iron, aluminum, gold, silver, and alloys thereof, which are used as conductors or terminal materials in conventional circuits and electronic circuits. The enameled wire can be not only an enameled copper wire, but also an enameled aluminum wire. The so-called contact between the enameled wire and the object to be bonded means that the enameled wire is in contact with a part of the object to be bonded. In addition, if the object to be bonded and the enameled wire are very close, they may not be in contact.

[0033] The flux of the present invention can be wetted by solder even if it is an enameled aluminum wire. Therefore, if the object to be joined is very close to the enameled wire, the object to be joined and the enameled wire can be electrically joined by solder. The distance is about 0.1 mm. That is, in the present invention, the situation of contacting and fixing the enameled wire and the object to be joined includes not only the situation of actual contact, but also the situation of placing the enameled wire and the object to be joined in close proximity. The object formed by the contact and fixing of the enameled wire and the object to be joined is called "the object to be joined".

[0034] Next, the object to be joined is immersed in the flux of the present invention. Here, the object to be joined only needs to be immersed in the flux at the portion where the object to be joined and the enameled wire are in contact and fixed. In other words, the portion to be welded between the enameled wire and the object to be joined is immersed in the flux.

[0035] Then, the object to be joined with the flux attached thereto is immersed in molten solder. When immersed in the molten solder, the flux may not be dried. That is, the object to be joined may be immersed in the flux and then immediately immersed in the molten solder.

[0036] In the step of immersing in molten solder, the object to be joined to which the flux is attached may not be kept in the molten solder for a while, but may be immediately pulled out after all the portions to which the flux is attached are immersed in the molten solder.

[0037] The dipping in flux and the dipping in molten solder can be performed not only once but also multiple times. That is, the object to be joined is dipped in flux and then dipped in molten solder. This is considered as a single set and can be performed multiple times. However, the flux of the present invention can weld the object to be joined consisting of enameled wire and the object to be joined by only one set of dipping the object to be joined in flux and then dipped in molten solder. The material of the welded object to be joined is called a "finished joined object".

[0038] The joining method using the flux of the present invention requires an operation of immersing the object to be joined with the flux attached thereto in solder. That is, the object to be joined is subjected to the action of the interface between the solder and the flux on its surface, while the enamel is peeled off and the solder wets the object to be joined.

[0039] After being immersed in the molten solder, the joined object can be cleaned. Since the flux of the present invention is composed of components with a boiling point below 400°C, all the components evaporate at the stage of being immersed in the molten solder. However, this is done to avoid corrosion of the joined object or the joined object in the event that the components constituting the flux remain.

[0040] In addition, the joining method using the flux of the present invention can also be used for joining enameled wires to electrical components or electronic components. That is, the object to be joined can be an electrical component or electronic component using enameled wires. In particular, it is suitable for joining enameled wires to terminals of components such as rotors or stators of electromagnets or motors, and inductors made by winding enameled wires. Example

[0041] In order to confirm the effect of the soldering flux of the present invention, the following experiment was performed. <Weldability test> After winding an enameled aluminum coil wire around a wiring terminal (0.64×0.64×20 mm, tin-plated on nickel), a test flux was applied and the wire was immersed in molten solder in a solder bath (soldering temperature: 400°C, solder composition: 96.1% tin-3.5% silver-0.4% nickel by mass).

[0042] Figure 1 The appearance of the samples used is shown. Figure 1 (a) is a rotor 10 of an electric motor. The rotor 10 is configured such that two wiring terminals 10b (10ba and 10bb) are mounted on a main body 10a formed of a cylindrical insulating material. Figure 1 (b) The enameled aluminum wire 12 is wound around the wiring terminal 10ba on one side. The enameled aluminum wire 12 is also wound around the main body 10a and is wound around the wiring terminal 10bb on the other side. Here, the wiring terminal 10b is the object to be joined 14, and the wiring terminal 10b with the enameled aluminum wire 12 wound therearound is the object to be joined 16.

[0043] Next, see Figure 2. First, the object to be joined 16 is immersed in the above-mentioned test flux 18 (P100). Then, the object to be joined 16 is immersed in the molten solder 20 prepared in the solder tank 20a (P102). The object to be joined 16 is pulled up from the molten solder 20 (P104). When the flux 18 of the present invention is used, the completed joined object 16a can be obtained by this single group (one step of immersing in the flux 18 and immersing in the solder 20) without any unwetted portion of the solder being generated at the portion of the object to be joined 16 that contacts the wiring terminal 10b to which the enameled aluminum wire 12 is fixed, and the solder is fully wetted.

[0044] The welded portion of the completed joint 16a was visually evaluated, with the case where the solder sufficiently wetted the wiring terminal 10b and the enameled aluminum wire 12 to form an integrated whole being recorded as "◎" (meaning excellent and qualified); the case where the wettability was slightly poor but sufficient for use as a product being recorded as "○" (meaning qualified); and the case where the wettability was insufficient and could not be used as a product being recorded as "×" (meaning unqualified).

[0045] In addition, an experiment was also conducted in which flux was applied to an aluminum plate that was not coated with enamel and then immersed in molten solder.

[0046] The composition of the test flux is shown below. (Example 1) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 1.

[0047] Among them, PINECRYSTAL KE-359 (also shown as "PCKE-359") was used as the rosin ester. PCKE-359 is a rosin derivative (rosin ester) produced by Arakawa Chemical Industries, Ltd. In addition, PhDG is diethylene glycol monophenyl ether, CHAH is cyclohexylamine hydrofluoride, and TAIC6B represents tris(2,3-dibromopropyl)isocyanurate.

[0048] (Example 2) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 2.

[0049] Among them, PINECRYSTAL KE-100 (also referred to as "PCKE-100") was used as the rosin ester. PCKE-100 is a rosin derivative (rosin ester) produced by Arakawa Chemical Industries, Ltd.

[0050] (Example 3) As rosin, 20.0% by mass of polymerized rosin and 25.0% by mass of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 3.

[0051] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester.

[0052] (Example 4) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% PhFG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 4.

[0053] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester. In addition, PhFG is propylene glycol monophenyl ether.

[0054] (Example 5) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 5.

[0055] As the rosin ester, PINECRYSTAL KE-311 (also referred to as "PCKE-311") was used. PCKE-311 is a rosin derivative (rosin ester) produced by Arakawa Chemical Industries, Ltd.

[0056] (Example 6) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 6.

[0057] As the rosin ester, PINECRYSTAL D-6011 (also referred to as "PCD-6011") was used. PCD-6011 is a rosin derivative (rosin ester) produced by Arakawa Chemical Industries, Ltd.

[0058] (Example 7) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 7.

[0059] Here, Ester Gum 105 (also referred to as "EG105") was used as the rosin ester. EG105 is a rosin derivative (rosin ester) produced by Arakawa Chemical Industries, Ltd.

[0060] (Example 8) As rosin, 40.0 mass % of purified rosin and 5.0 mass % of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 8.

[0061] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester.

[0062] (Example 9) As rosin, 10.0 mass % of purified rosin and 45.0 mass % of rosin ester were used. 41.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials are mixed to prepare the soldering flux of Example 9.

[0063] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester.

[0064] (Comparative Example 1) As rosin, 45.0 mass% of purified rosin, 51.7 mass% PhFG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials were mixed to prepare the flux of Comparative Example 1.

[0065] However, Comparative Example 1 does not contain rosin ester.

[0066] (Comparative Example 2) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% IPA as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials were mixed to prepare the flux of Comparative Example 2.

[0067] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester. IPA is isopropyl alcohol.

[0068] (Comparative Example 3) As rosin, 20.0 mass% of purified rosin and 25.0 mass% of rosin ester, 51.7 mass% BZA as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials were mixed to prepare the flux of Comparative Example 3.

[0069] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester. In addition, BZA is benzyl alcohol.

[0070] (Comparative Example 4) As rosin, 44.0 mass% of purified rosin and 1.0 mass% of rosin ester, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials were mixed to prepare the flux of Comparative Example 4.

[0071] Among them, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester.

[0072] (Comparative Example 5) As 45.0 mass% of rosin ester of rosin, 51.7 mass% PhDG as solvent, 2.3 mass% CHAH as active agent, 1.0 mass% TAIC6B as a co-active agent, The above materials were mixed to prepare the flux of Comparative Example 5. Comparative Example 5 did not contain rosin other than rosin ester.

[0073] Here, PINECRYSTAL KE-359 (PCKE-359) was used as the rosin ester. In addition, the rosin of Comparative Example 5 consisted of only the rosin ester.

[0074] Table 1 shows the composition of each sample of the embodiment and the evaluation of the experimental results. In addition, Table 2 shows the composition of each sample of the comparative example and the evaluation of the experimental results. In the table, the embodiment is also shown as "Ex" and the comparative example is shown as "CEx".

[0075] Table 1

[0076] Table 2

[0077] Referring to Comparative Example 1, the solder wetted well the uncoated aluminum plate, but hardly wetted the enameled aluminum wire (recorded as "enameled aluminum coil wire" in the table). That is, cyclohexylamine hydrofluoride (CHAH) as an activator and tris(2,3-dibromopropyl)isocyanurate (TAIC6B) as an auxiliary activator wetted aluminum well, but the purified rosin could not strip the enameled coating and could not wet the solder well.

[0078] On the other hand, referring to Examples 1 and 2, solder wetting was good not only for the uncoated aluminum plate but also for the enameled aluminum wire. That is, the enameling can be stripped by rosin esters such as PINECRYSTAL KE-359 and PINECRYSTAL KE-100.

[0079] In addition, referring to Examples 3 and 5 to 7, as long as rosin esters such as PINECRYSTAL KE-359, PINECRYSTAL KE-100, PINECRYSTAL KE-311, PINECRYSTAL D-6011, and Ester Gum 105 are contained, the enamel can be stripped and the solder can be well wetted even if other rosins such as purified rosin or polymerized rosin are used as the rosin added.

[0080] Referring to Comparative Examples 2 and 3, solvents having a boiling point lower than the melting point of lead-free solder, such as isopropyl alcohol (IPA: boiling point 82.4°C) or benzyl alcohol (BZA: boiling point 206°C), evaporate instantly due to the heating during soldering, and evaporate before the enamel is stripped, making it impossible to strip the enamel and failing to wet the solder well.

[0081] On the other hand, referring to Examples 1 and 4, a phenyl group-containing glycol solvent such as diethylene glycol monophenyl ether or propylene glycol monophenyl ether (PhFG) can strip the enamel and wet the solder well.

[0082] Referring to Examples 8 and 9, the effect of the present invention can be achieved when the rosin ester is 5% by mass or more and 45% by mass or less relative to the total amount of the flux. In this case, it is preferred that the content of other rosins is 10% by mass relative to the total amount of the flux (Example 9). When the rosin ester is less than 5% by mass relative to the total amount of the flux, the enameled aluminum coil wire cannot be wetted (as can be seen from the comparison between Example 8 and Comparative Example 4).

[0083] In addition, all the examples were evaluated as "◎" (which means excellent and acceptable) for the enameled copper wire. Industrial Applicability

[0084] As described above, the flux of the present invention can be suitably used for soldering enameled wires even when the enameled wires are not peeled off. In addition, the wires in this case may be made of copper or aluminum. Explanation of symbols

[0085] 10 rotors 10a Main body 10b wiring terminal 12 enameled aluminum wire 14 Object to be bonded 16Joining the predetermined object 16a Joining completed object 18. Flux 20 molten solder 20a solder bath 22 Solder unwetted part

Claims

1. A soldering flux comprising: Rosin esters, Rosin other than the rosin ester, At least one of diethylene glycol monophenyl ether and propylene glycol monophenyl ether as a solvent, and Organic hydrofluoride (as active agent).

2. The soldering flux according to claim 1, characterized in that The organic hydrofluoric acid salt is at least one of cyclohexylamine hydrofluoric acid salt, 1,3-diphenylguanidine hydrofluoric acid salt, N,N'-diethylaniline hydrofluoric acid salt, and diethylamine hydrofluoric acid salt.

3. The soldering flux according to claim 1 or 2, characterized in that The invention further contains at least one of 2,3-dibromo-1-propanol, 1,2,5,6,9,10-hexabromocyclododecane, tris(2,3-dibromopropyl)isocyanurate and 2,2-bis(4-bromomethyl)-1,3-propanediol as an auxiliary active agent.

4. The soldering flux according to any one of claims 1 to 3, wherein The rosin is 20 mass % to 55 mass % relative to the total amount of the flux. The rosin ester is 5% to 45% by mass relative to the total amount of the flux. The other rosin is greater than or equal to 10 mass % based on the total amount of the soldering flux.

5. A method for welding enameled wire, characterized in that: The process of contacting and fixing the enameled wire with the object to be joined to form a predetermined object to be joined, a step of immersing the objects to be joined in the flux according to any one of claims 1 to 3, and The step of immersing the object to be joined in molten solder to form a joined object in which the enameled wire and the object to be joined are fused together.

6. The method for welding enameled wires according to claim 4, characterized in that: The method comprises the step of washing the bonded product.