Resin composition for sliding and sliding member
By rationally combining resin and inorganic materials in the sliding parts of the submersible pump, the problem of poor balance between sliding properties and linear expansion coefficients is solved, and sliding parts with low friction, low wear and high mechanical strength are achieved, which are suitable for various purposes.
Patent Information
- Application Number
- CN202380023467.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2023-02-27
- Publication Date
- 2024-10-15
AI Technical Summary
During use, the sliding parts of existing submersible pumps have a poor balance between sliding properties and linear expansion coefficients, resulting in severe wear, increased friction coefficients, reduced mechanical strength, and the inability to maintain the expected dimensional accuracy and heat resistance.
By rationally combining resin components, uncarbonized carbon fibers and inorganic materials in the sliding resin composition, the friction coefficient, wear amount and linear expansion coefficient are controlled, and a specific firing temperature and tensile elastic modulus range are adopted to ensure the long-term durability of the sliding parts. Excellent performance.
It achieves low friction coefficient, low wear amount and low linear expansion coefficient of sliding parts, ensuring a balance between sliding properties and mechanical strength, extending the service life of parts and maintaining dimensional accuracy.
Smart Images

Figure CN118786185A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a sliding resin composition and a sliding part.
[0002] More specifically, the present invention relates to a sliding resin composition which can provide a sliding part having a good balance between sliding properties and linear expansion coefficient, etc., by blending a predetermined amount of an inorganic material, and a sliding part obtained from such a sliding resin composition. Background Art
[0003] Existing submersible pumps are used for various purposes, such as water pumping devices for pumping water from rivers and oceans, and water circulation in water heaters, floor heating equipment, automobile engines, inverters, batteries or fuel cells, etc.
[0004] An example of the submersible pump (water pump) includes the following structures 1) to 5) including a predetermined sliding member (sliding bearing, thrust receiving member) (for example, refer to Patent Document 1).
[0005] 1) Impeller
[0006] 2) Shaft for fixing the impeller
[0007] 3) Sliding bearing fixed to the impeller, which is used to support the impeller to rotate freely relative to the shaft support
[0008] 4) Thrust bearing components that slide with the end faces of the sliding bearing
[0009] 5) The casing and cover that contain the impeller and form the pump chamber
[0010] The sliding bearing, which is a sliding component, is a cylindrical bearing that receives loads on the inner diameter and the end surface and has the same thickness on the end surface, and is an injection molded product made of a resin composition having a linear polyphenylene sulfide resin as a base resin.
[0011] That is, it is an injection molded product derived from a resin composition comprising carbon fibers which are carbides sintered at 1000 to 1500° C. and at least one selected from a polytetrafluoroethylene resin and graphite in a predetermined base resin.
[0012] Furthermore, there has been proposed a sliding part using, as a reinforcing material, predetermined uncarbonized carbonaceous fibers different from the uncarbonized carbon fibers of the present invention (for example, see Patent Document 2).
[0013] More specifically, the sliding member is a sintered body obtained by sintering a composite body having a predetermined shape and composed of the following blending components 1) to 3).
[0014] For example, the raw material pitch is supplied to a spinner, heated to 300-400°C, and extruded from a nozzle under the pressure of an inert gas to obtain raw material fibers. Subsequently, the obtained raw material fibers are maintained in an oxidizing atmosphere at about 150-500°C for about 0.5-5 hours to be insolubilized to obtain carbon fibers, which are used as sliding parts containing a specified amount of uncarbonized carbonaceous fibers.
[0015] 1) Uncarbonized carbon fibers heat treated at a temperature below 550°C
[0016] 2) Boron compounds and other inorganic powders or inorganic fibers
[0017] 3) Inorganic powder or its inorganic fiber having self-sintering properties in which uncarbonized carbonaceous fibers and boron compounds are embedded
[0018] It should be noted that uncarbonized carbonaceous fibers are carbonaceous fibers that have not been subjected to carbonization treatment at a normal temperature, and are defined as carbonaceous fibers that have been heat-treated (burned) at a temperature of 550° C. or less and still have room for further carbonization.
[0019] Furthermore, according to the embodiment of Patent Document 2, the composites composed of 1) to 3) are all heated to 1000°C in a non-oxidizing atmosphere or a nitrogen atmosphere at normal pressure for primary sintering, and further heated to 1300°C, 1700°C or 2000°C in the atmosphere for secondary sintering. Therefore, the uncarbonized carbonaceous fibers of Patent Document 2 are finally heat-treated at a temperature substantially above 1000°C.
[0020] [Prior art literature]
[0021] [Patent Document]
[0022] [Patent Document 1] Japanese Patent No. 6639592 (claims, etc.)
[0023] [Patent Document 2] Japanese Patent Application Laid-Open No. 3-237062 (claims, etc.) Summary of the invention
[0024] However, the sliding component (sliding bearing, etc.) used for the submersible pump (water pump) described in Patent Document 1 is characterized in that carbide fired at 1000 to 1500° C. is used as reinforcing fiber for a predetermined resin.
[0025] Therefore, there is a problem that the balance between the sliding property and the linear expansion coefficient of the sliding member is poor.
[0026] That is, in order to obtain the desired linear expansion coefficient, if a large amount of conventional carbides (hereinafter sometimes referred to as carbonized carbon fibers), graphitized carbon fibers or inorganic fillers are added to the resin component, the following tendency is observed: as time passes, wear in the sliding parts becomes more severe, and as a result, it is observed that the carbon fibers, inorganic fillers, etc. are easily exposed on the surface.
[0027] As a result, the friction coefficient of the sliding part increases or the counterpart part is damaged, which significantly reduces the sliding property. In addition, excessive heat is generated, exceeding the heat resistance of the resin component, and melting occurs.
[0028] On the other hand, if the amount of carbonized carbon fiber, graphitized carbon fiber or inorganic filler mixed in the past is reduced relative to the resin component, the mechanical strength of the sliding parts will decrease, the wear will increase, the linear expansion coefficient of the sliding parts will increase, the dimensional change caused by sliding heat will increase, and the desired dimensional accuracy will not be maintained.
[0029] In addition, the sliding member described in Patent Document 2 needs to use uncarbonized carbonaceous fibers fired at an extremely low temperature, and has a problem in that it is difficult to maintain good sliding properties and a low linear expansion coefficient.
[0030] That is, for example, it is necessary to use uncarbonized carbonaceous fibers obtained by extruding raw material pitch from a nozzle at 300-400°C under inert gas pressure, and then maintaining the raw material pitch at about 150-500°C for about 0.5-5 hours in an oxidizing atmosphere.
[0031] This is to improve the interface adhesion with the self-sintering carbonaceous powder. Ultimately, if the temperature is not raised to 1000°C in a non-oxidizing atmosphere or a nitrogen atmosphere at normal pressure for primary sintering as described above, and then the temperature is not raised to 1300°C, 1700°C or 2000°C in the atmosphere for secondary sintering, the desired strength cannot be obtained.
[0032] Moreover, the sliding part described in Patent Document 2 is an invention related to a reinforced carbon composite material based on carbon fibers, the so-called C / C composite material. Therefore, there is no description or consideration at all about the situation of combining the uncarbonized carbonaceous fibers described in Patent Document 2 with a resin composition.
[0033] In view of this, the inventors conducted intensive studies and found that, in a sliding resin composition, by adding a predetermined uncarbonized carbon fiber as a compounding component (b) and an inorganic material as a compounding component (c) at a predetermined ratio to a resin component as a compounding component (a), a low friction coefficient and a small wear amount can be obtained while maintaining a low linear expansion coefficient when processed into a sliding part, thereby completing the present invention.
[0034] That is, an object of the present invention is to provide a sliding resin composition and a sliding part obtained from the sliding resin composition, wherein the sliding resin composition comprises at least compounded components (a) to (c) and when processed into a sliding part, can obtain a sliding part that exhibits excellent sliding properties for a long period of time.
[0035] According to the present invention, there is provided a sliding resin composition characterized by containing the following blending components (a) to (c), thereby being able to solve the above-mentioned problems.
[0036] (a) Resin component: 100 parts by weight
[0037] (b) 5 wt% uncarbonized carbon fibers with a reduction temperature of 400 to 550°C: 10 to 400 parts by weight
[0038] (c) Inorganic materials: 10 to 80 parts by weight
[0039] Thus, in the sliding resin composition, the resin component (a), the uncarbonized carbon fibers having a 5 wt% reduction temperature (hereinafter sometimes referred to as TG5) within a predetermined range as a thermogravimetric measurement under predetermined conditions as a compounding component (b), and the inorganic material as a compounding component (c) are compounded in predetermined ratios, respectively. When the composition is processed into a sliding part, the friction coefficient, the wear amount, and the linear expansion coefficient are respectively below the predetermined values, thereby achieving good sliding performance.
[0040] When the sliding resin composition of the present invention is constituted, the tensile modulus of the component (b) measured in accordance with JIS R7606:2000 is preferably a value within the range of 10 to 35 GPa.
[0041] Thus, in the sliding resin composition, by specifying the tensile modulus of the uncarbonized carbon fibers as the compounding component (b), the linear expansion coefficient is set to a specified value or less when processed into a sliding part, thereby enabling excellent sliding properties to be exhibited for a long period of time.
[0042] When the sliding resin composition of the present invention is formed, the tensile elongation of the component (b) as measured in accordance with JIS R7606:2000 is preferably within a range of 2 to 5%.
[0043] Thus, in the sliding resin composition, by specifying the tensile elongation of the uncarbonized carbon fibers as the compounding component (b), the linear expansion coefficient is set to a specified value or less when processed into a sliding part, thereby enabling excellent sliding properties to be exhibited for a long period of time.
[0044] When the sliding resin composition of the present invention is constituted, the carbon content of the surface of the blended component (b) as determined by XPS elemental analysis is preferably within a range of 85 to 96% by weight relative to the total weight.
[0045] Thus, in the sliding resin composition, by regulating the carbon content of the compounded component (b) to a value within a predetermined range, when processed into a sliding part, excellent sliding properties can be more quantitatively exhibited for a long period of time.
[0046] In addition, when the sliding resin composition of the present invention is formed and processed into a sliding part, the linear expansion coefficient measured in accordance with JIS K7197:2012 is preferably 5×10 -5 / ℃ below.
[0047] By making the linear expansion coefficient of the sliding part made from the sliding resin composition be a predetermined value or less in this way, it is possible to further provide quantitative properties and to easily and stably form a sliding part adapted to various uses.
[0048] When the sliding resin composition of the present invention is constituted, it is preferred that the weight ratio of the compounded component (b) / the compounded component (c) be a value within a range of 1 / 1 to 10 / 1.
[0049] By limiting the weight ratio of the compounded component (b) / the compounded component (c) in the sliding resin composition, it is easier to adjust the friction coefficient and the linear expansion coefficient to values below the prescribed values when processing into sliding parts.
[0050] When the sliding resin composition of the present invention is constituted, the compounded component (a) is preferably at least one selected from the group consisting of polyphenylene sulfide resins, polyethersulfone resins, polyetheretherketone resins, polyimide resins, and thermosetting phenol resins.
[0051] By specifying the type of the blended component (a) in this manner, the heat resistance can be improved and the linear expansion coefficient can be reduced.
[0052] Therefore, by limiting the type of resin component, when processed into a sliding part, the material has good heat resistance and processability, and can stably exhibit excellent performance such as a friction coefficient and a linear expansion coefficient being below a specified value for a long period of time.
[0053] Another aspect of the present invention is a sliding component characterized in that the linear expansion coefficient measured in accordance with JIS K 7197:2012 is 5×10 -5 / °C or less, which is derived from a sliding resin composition containing the following compounding components (a) to (c).
[0054] (a) Resin component: 100 parts by weight
[0055] (b) 5 wt% uncarbonized carbon fibers with a reduction temperature of 400 to 550°C: 10 to 400 parts by weight
[0056] (c) Inorganic materials: 10 to 80 parts by weight
[0057] In this way, by making the sliding part from a sliding resin composition in which uncarbonized carbon fibers having a 5 wt % reduction temperature based on thermogravimetric measurement within a predetermined range are added as a compounding component (b) to the resin component as a compounding component (a), the linear expansion coefficient is small and excellent sliding properties can be exhibited for a long time. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 (a) to (c) are graphs provided to explain the relationship between the firing temperature of carbon fibers and the linear expansion coefficient, friction coefficient, and wear amount of sliding parts.
[0059] Figure 2 This is a diagram for explaining the relationship between the calcination temperature of carbon fibers and the 5 wt% reduction temperature (TG5) of carbon fibers.
[0060] Figure 3 (a) to (b) are graphs provided for explaining the relationship between the calcination temperature of carbon fiber and the tensile elastic modulus and tensile elongation of carbon fiber, respectively.
[0061] Figure 4 This is a diagram for explaining the relationship between the calcination temperature of carbon fibers and the volume resistivity (logarithmic expression) of carbon fibers.
[0062] Figure 5 (a) to (c) are graphs provided to explain the relationship between the blending amount of uncarbonized carbon fibers and the linear expansion coefficient, friction coefficient, and wear amount of a sliding component.
[0063] Figure 6 (a) to (c) are graphs provided to illustrate the relationship between the weight ratio of uncarbonized carbon fiber as compounding component (b) / compounding component (c), i.e., inorganic material, and the linear expansion coefficient, friction coefficient, and wear amount in the sliding component.
[0064] Figure 7 (a) corresponds to Example 1 of the present invention, Figure 7 (b) corresponds to Comparative Example 2 of the present invention, and is a cross-sectional photograph (magnification: 500) for explaining the dispersion state of the compounding component (b) of the sliding resin composition. DETAILED DESCRIPTION
[0065] [First embodiment]
[0066] The first embodiment is a sliding resin composition characterized by containing the following compounding components (a) to (c).
[0067] (a) Resin component: 100 parts by weight
[0068] (b) 5 wt% uncarbonized carbon fibers with a reduction temperature of 400 to 550°C: 10 to 400 parts by weight
[0069] (c) Inorganic materials: 10 to 80 parts by weight
[0070] That is, Figure 1 As shown in (a) to (c), in order to control the linear expansion coefficient, friction coefficient and wear amount of the sliding parts made of the sliding resin composition, as shown in Figure 2 As shown, a sliding resin composition is prepared by mixing carbon fibers (uncarbonized carbon fibers) having a predetermined 5% weight reduction temperature (TG5) measured by a thermogravimetric analyzer (TGA).
[0071] The sliding resin composition is obtained by mixing a predetermined amount of such uncarbonized carbon fibers as a compounding component (b) and an inorganic material as a compounding component (c) into a resin component as a compounding component (a).
[0072] Hereinafter, the sliding resin composition of the first embodiment will be described in more detail with reference to the drawings as appropriate, mainly focusing on the compounding components (a) to (c) and the like constituting the composition.
[0073] 1. Compounding ingredients (a)
[0074] (1) Types
[0075] The type of the resin component as the compounded component (a) is not particularly limited, and any known resin component used for sliding parts can be appropriately used.
[0076] More specifically, among such known resin components, at least one heat-resistant resin selected from the group consisting of polyphenylene sulfide resin (PPS), polyethersulfone resin (PES), polyetheretherketone resin (PEEK), polyimide resin (PI) and thermosetting phenolic resin (PF) is preferred.
[0077] The reason for this is that these heat-resistant resins generally have a continuous use time of, for example, 40,000 hours as heat resistance and a continuous use temperature of 150° C. or higher. Therefore, even when the ambient temperature rises, good mechanical strength, sliding properties, etc. can be maintained over time.
[0078] Furthermore, since these heat-resistant resins have relatively low water absorption, even when used for sliding parts of submersible pumps, the sliding parts (such as sliding bearings) experience little dimensional change and exhibit good sliding properties.
[0079] It should be noted that the resin component (heat-resistant resin) as the compounding component (a) can be used as the main component. As a standard, when the total amount of the resin component is set to 100 weight %, it is preferably 50 weight % or more, more preferably 70 weight % or more, and further preferably 90 weight % or more.
[0080] Moreover, as the compounding component (a), among these heat-resistant resins, polyphenylene sulfide resin (including modified products of polyphenylene sulfide resin, sometimes referred to as PPS resin) is a more suitable resin component.
[0081] The reason is that PPS resin is generally a crystalline, translucent thermoplastic resin with a high melting point of about 280°C and a glass transition temperature of 93°C. It has extremely high rigidity, excellent heat resistance, dimensional stability, abrasion resistance, low water absorption, etc.
[0082] Furthermore, the PPS resin has a low melt viscosity and can be added with a large amount of uncarbonized carbon fibers and inorganic materials, which is excellent in productivity.
[0083] In addition, PPS resins are classified into a cross-linked type, a linear type, and a semi-cross-linked type according to their molecular structures, and each of these types can be used alone or in combination of two or more types.
[0084] Furthermore, in order to form a sliding bearing that takes into account abrasive wear forms such as a water-repellent state where no water film is formed or a state where foreign matter is bitten, a straight-chain type having toughness is also preferred among PPS resins.
[0085] (2) Quantity
[0086] The amount of the resin component as the compounding component (a) can be determined in consideration of the heat resistance, moldability, mechanical strength, etc. of the obtained sliding part. Generally, the compounding amount of the compounding component (a) is preferably set to a value in the range of 10 to 80 wt % relative to the total amount (100 wt %) of the sliding resin composition.
[0087] The reason is that when the amount of the compounding component (a) is less than 10% by weight, the amount of the uncarbonized carbon fiber (for example, a calcined product at 600 to 800° C.) as the compounding component (b) and the inorganic material (talc, etc.) as the compounding component (c) increases, and the melt viscosity of the sliding resin composition becomes too high, which deteriorates the molding processability and sometimes makes it difficult to obtain a sliding part that exhibits excellent sliding properties.
[0088] On the other hand, if the amount of the compounding component (a) is greater than 80% by weight, the amount of the uncarbonized carbon fiber as the compounding component (b) and the inorganic material as the compounding component (c) is reduced, and the adjustment of the linear expansion coefficient of the obtained sliding part becomes difficult, and the mechanical strength, etc. are significantly reduced, and sometimes the excellent sliding property cannot be exerted.
[0089] Therefore, the amount of the component (a) added is more preferably within a range of 15 to 60% by weight, and even more preferably within a range of 20 to 50% by weight, relative to the total amount of the sliding resin composition.
[0090] 2. Compounding ingredients (b)
[0091] (1) 5% weight reduction temperature based on thermogravimetric measurement
[0092] In the specified uncarbonized carbon fiber as the compounding component (b), it is characterized in that the 5 weight % reduction temperature (hereinafter sometimes referred to as TG5) measured using TGA under the conditions of an air flow rate of 100 ml / min and a heating rate of 5°C / min is a value in the range of 400 to 550°C.
[0093] The reason for this is that when the TG5 is less than 400°C, heat resistance, mechanical strength, etc. are excessively reduced, and when processed into a sliding part, the durability is significantly reduced.
[0094] On the other hand, if TG5 exceeds 550°C, the heat resistance and mechanical strength of the steel itself are improved, but the friction coefficient increases when processed into a sliding part.
[0095] Therefore, it is more preferable that the TG5 of the uncarbonized carbon fibers be a value within a range of 430 to 500°C, and further preferably a value within a range of 450 to 490°C.
[0096] In addition, this TG5 can be measured using TGA, and in the obtained weight reduction graph, the temperature at which the weight is reduced by 5% by weight from the initial weight (100% by weight) is used as a reference.
[0097] In addition, the TG5 of the uncarbonized carbon fibers can be basically controlled to a value within a predetermined range by controlling the firing temperature to be relatively low.
[0098] That is, the carbide described in Patent Document 1 and the like in the prior art is a carbon fiber sintered at least at 1000°C, preferably 1300 to 1500°C, and it has been separately found that its TG5 exceeds 700°C.
[0099] In addition, the uncarbonized carbonaceous fibers described in Patent Document 2 of the prior art are fired at a temperature of 500°C or lower, and it is separately found that the carbonization degree is quite low, and the TG5 thereof is less than 400°C.
[0100] Therefore, when producing the predetermined uncarbonized carbon fibers as the compounding component (b), it can be said that it is generally preferred to set the calcining temperature to a range of 600 to 800°C.
[0101] Therefore, for the uncarbonized carbon fiber TG5 specified as the compounding component (b), its carbonization degree is higher than that of the uncarbonized carbonaceous fibers fired at a temperature below 500°C, and on the other hand, it is lower than that of the carbides fired at a temperature above 1000°C, and is a low-temperature carbide that is clearly different from these carbon fibers.
[0102] That is, as described later, the uncarbonized carbon fibers containing component (b) are observed to have significant property differences from uncarbonized carbon fibers (low-temperature carbides) and carbides in terms of tensile elastic modulus, tensile elongation, XPS surface element analysis (carbon content), volume resistivity, saturated moisture content, etc., and can be clearly distinguished.
[0103] Here, refer to Figure 2 , the relationship between the calcination temperature of carbon fiber (including uncarbonized carbon fiber and other carbon fiber, the same below) and the 5 weight % reduction temperature (TG5) caused by TGA, which is one of its thermal decomposition temperatures, is explained.
[0104] Right now, Figure 2 The horizontal axis is represented by the sintering temperature (° C.) of the carbon fiber, and the vertical axis is represented by the TG5 value (° C.) of the carbon fiber.
[0105] As described later, Figure 2 The characteristic curves in FIG. 1 are the results of TG5 of carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2, which differed only in the firing temperature.
[0106] In addition, in the drawings, Example 1 is described as Example 1 and Comparative Example 1 is described as Comparative Example 1, and the same shall apply hereinafter.
[0107] By this Figure 2 As can be seen from the characteristic curve in , the lower the sintering temperature of the carbon fiber, the more accurately the TG5 value corresponds and tends to become lower, that is, there is a tendency to be proportional.
[0108] More specifically, when the sintering temperature of the carbon fiber is greater than 1200°C, TG5 is greater than 550°C, but when the sintering temperature of the carbon fiber is 600-800°C, TG5 is a value in the range of 400-550°C, and when the sintering temperature of the carbon fiber is less than 600°C, TG5 is sometimes less than 400°C.
[0109] Therefore, according to Figure 2 Judging from the results of the characteristic curve shown, it can be said that by adjusting the sintering temperature of the carbon fiber to a predetermined range, the TG5 of the carbon fiber can be accurately controlled to a predetermined temperature.
[0110] (2) Morphology
[0111] In addition, the average fiber diameter (average diameter) of the uncarbonized carbon fibers used as the compounding component (b) is usually 30 μm or less, preferably a value in the range of 3 to 25 μm, and more preferably a value in the range of 5 to 20 μm, which can be appropriately determined depending on the application, ease of use, etc.
[0112] Similarly, the average length of the uncarbonized carbon fibers of component (b) is usually 500 μm or less, preferably 50 to 450 μm, and more preferably 100 to 400 μm, but this can be appropriately determined depending on the application, ease of use, etc.
[0113] (3) Tensile elastic modulus
[0114] Furthermore, the tensile elastic modulus of the uncarbonized carbon fibers as the compounding component (b) is usually preferably a value within the range of 10 to 35 GPa.
[0115] The reason for this is that if the tensile modulus is a value less than 10 GPa, the mechanical strength and wear resistance may be significantly reduced when processed into a sliding part.
[0116] On the other hand, if the tensile elastic modulus exceeds 35 GPa, the friction coefficient of the obtained sliding member may increase.
[0117] Therefore, the tensile modulus of the blended component (b) is more preferably set to a value within the range of 13 to 30 GPa, and further preferably set to a value within the range of 16 to 25 GPa.
[0118] It should be noted that the tensile modulus of the uncarbonized carbon fibers can be measured in accordance with JIS R 7606:2000.
[0119] Here, refer to Figure 3 (a) The relationship between the calcination temperature and the tensile modulus of carbon fibers (including uncarbonized carbon fibers and other carbon fibers) is described.
[0120] Right now, Figure 3 The horizontal axis of (a) represents the sintering temperature (° C.) of the carbon fiber, and the vertical axis represents the value of the tensile elastic modulus (GPa) of the carbon fiber.
[0121] Furthermore, as described later, Figure 3The characteristic curve in (a) is based on the tensile elastic modulus of the carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2, which differ only in the firing temperature.
[0122] Depend on Figure 3 From the characteristic curve in (a), it can be seen that the value of the tensile modulus of the carbon fiber tends to significantly increase as the sintering temperature of the carbon fiber increases.
[0123] More specifically, when the carbon fiber is fired at a temperature lower than 600° C., the tensile modulus is lower than 10 GPa, and when the carbon fiber is fired at a temperature of 450° C., the tensile modulus is a relatively low value lower than 1 GPa.
[0124] It was also found that when the carbon fiber is fired at a temperature of 600 to 800°C, the tensile modulus reaches a value of at least 10 GPa, and when other manufacturing conditions (stretching conditions, firing time) are changed, a maximum value of about 35 GPa is obtained.
[0125] Furthermore, when the sintering temperature of the carbon fibers is higher than 1200° C., the tensile modulus becomes a value higher than 35 GPa.
[0126] Therefore, it can be said that by adjusting the firing temperature of the carbon fibers to a predetermined range, the tensile modulus of the carbon fibers can be reliably controlled to a value within a desired range.
[0127] (4) Tensile elongation
[0128] Furthermore, the tensile elongation of the uncarbonized carbon fibers as the compounding component (b) is usually preferably a value within the range of 2 to 5%.
[0129] The reason for this is that if the tensile elongation is a value less than 2%, the friction coefficient of the obtained sliding member may increase.
[0130] On the other hand, if the tensile elongation is greater than 5%, the mechanical strength and wear resistance may be significantly reduced when the sliding part is processed.
[0131] Therefore, the tensile elongation is more preferably set to a value within the range of 2.1 to 4%, and further preferably set to a value within the range of 2.2 to 3%.
[0132] It should be noted that the tensile elongation of the uncarbonized carbon fibers can be measured in accordance with JIS R 7606:2000.
[0133] Here, combined Figure 3 (b) The relationship between the calcination temperature and the tensile elongation of carbon fibers (including uncarbonized carbon fibers and other carbon fibers) is described.
[0134] Right now, Figure 3The horizontal axis of (b) represents the calcination temperature (°C) of the carbon fiber, and the vertical axis represents the tensile elongation value (%) of the carbon fiber.
[0135] Furthermore, as described later, Figure 3 The characteristic curve in (b) is based on the tensile elongation of carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2 that differ only in the firing temperature.
[0136] From this Figure 3 It can be understood from the characteristic curve described in (b) that when the calcination temperature of the carbon fiber is at least less than 600° C., the value of the tensile elongation of the carbon fiber tends to become significantly smaller as the calcination temperature becomes lower.
[0137] More specifically, when the calcination temperature of the carbon fibers is lower than 600° C., the tensile elongation becomes a value significantly lower than 2%.
[0138] It was also found that when the carbon fiber is fired at a temperature of 600 to 800°C, the tensile elongation reaches at least 2% and when other manufacturing conditions (stretching conditions, firing time) are changed, a maximum value of 5% can be achieved.
[0139] Furthermore, when the sintering temperature of the carbon fiber exceeds 800° C., the tensile elongation becomes a small value less than 2%.
[0140] Therefore, it can be said that by adjusting the calcining temperature of the carbon fibers to a predetermined range, the value of the tensile elongation of the carbon fibers can be accurately controlled to a value within a desired range.
[0141] (5) XPS surface element analysis (carbon content)
[0142] Furthermore, the carbon content of the surface of the uncarbonized carbon fibers as the blending component (b) as determined by XPS elemental analysis is preferably set to a value within a range of 85 to 96 wt % relative to 100 wt % of the total amount.
[0143] The reason is that by regulating the carbon amount on the surface based on XPS elemental analysis to a value within a prescribed range, unlike conventional carbides and uncarbonized carbonaceous fibers, a sliding resin composition having a friction coefficient, a wear amount, and a linear expansion coefficient each below a prescribed value can be more easily and stably provided when processed into a sliding part.
[0144] More specifically, when the carbon content based on XPS elemental analysis is a value less than 85% by weight, the mechanical strength, wear resistance, etc. of the sliding part may be significantly reduced.
[0145] On the other hand, when the carbon content based on XPS elemental analysis is a value exceeding 96% by weight, the friction coefficient may increase.
[0146] Therefore, the carbon content based on XPS elemental analysis is more preferably set to a value within a range of 86 to 95% by weight, and further preferably set to a value within a range of 88 to 94% by weight, based on the total amount.
[0147] It should be noted that the carbon content can be measured according to the XPS elemental analysis method based on a standard curve of the carbon element.
[0148] (6) Volume resistivity
[0149] The volume resistivity of the uncarbonized carbon fiber as the compounding component (b) is usually preferably 1×10 0 ~1×10 4 The value is within the range of Ω·cm.
[0150] The reason for this is that by regulating the volume resistivity to a value within a predetermined range, when processed into a sliding part, unlike conventional carbides and uncarbonized carbonaceous fibers, a sliding part having excellent electrical insulation, antistatic properties, etc. can be provided more easily and quantitatively stably.
[0151] More specifically, if the volume resistivity is less than 1×10 0 The value of Ω·cm is lower than that of Ω·cm, and the antistatic property becomes good, but the electrical insulation in the sliding part becomes insufficient, and problems such as spark generation outside may occur.
[0152] On the other hand, if the volume resistivity is greater than 1×10 4 If the value of Ω·cm is less than 0.04, the electrical insulation property becomes good, but static electricity may accumulate in the sliding parts, and the antistatic property may become insufficient.
[0153] Therefore, it is more preferable to set the volume resistivity of the uncarbonized carbon fibers to 5×10 0 ~5×10 3 The value is preferably within the range of Ω·cm, and more preferably 1×10 1 ~1×10 3 The value is within the range of Ω·cm.
[0154] Note that the volume resistivity of the uncarbonized carbon fibers can be measured by a four-terminal method using a commercially available digital voltmeter or the like.
[0155] Here, combined Figure 4 , the relationship between the sintering temperature and volume resistivity of carbon fibers (including uncarbonized carbon fibers and other carbon fibers) is described.
[0156] Right now, Figure 4 The horizontal axis is represented by the sintering temperature (° C.) of the carbon fiber, and the vertical axis is represented by the volume resistivity value (Ω·cm) of the carbon fiber.
[0157] Furthermore, as described later, Figure 4 The characteristic curves in FIG. 1 are based on the volume resistivity of the carbon fibers used in Examples 1 to 3 and Comparative Examples 1 and 2 in which only the sintering temperatures of the carbon fibers were different.
[0158] Depend on Figure 4 From the characteristic curve in FIG, it can be seen that the higher the sintering temperature of the carbon fiber, the more rapidly the volume resistivity tends to decrease.
[0159] More specifically, if the sintering temperature of carbon fiber is lower than 600°C, the volume resistivity becomes significantly greater than 1×10 4 The value of Ω·cm.
[0160] In addition, when the sintering temperature of carbon fiber is 600 to 800°C, the volume resistivity can be 1×10 0 ~1×10 4 The value is within the range of Ω·cm.
[0161] Furthermore, when the sintering temperature of carbon fiber exceeds 1200°C, the volume resistivity becomes less than 1×10 -1 Small value of Ω·cm.
[0162] Therefore, by adjusting the sintering temperature of the carbon fiber to a predetermined range, the volume resistivity value can be accurately controlled to a value within the predetermined range, thereby facilitating handling, and further, it can be said that desired antistatic properties and the like can be obtained in a predetermined sliding component.
[0163] (7) Saturated moisture content
[0164] The saturated moisture content of the uncarbonized carbon fibers as the compounding component (b) can be measured according to JIS K 7209:2000 which prescribes the method for determining the water absorption rate in plastics. Generally, the saturated moisture content of the uncarbonized carbon fibers is preferably within a range of 1 to 8 wt %.
[0165] The reason for this is that by regulating the saturated water content to a value within a predetermined range, when the material is processed into a sliding part or used for a bearing for a submersible pump, etc., excellent sliding properties can be obtained more easily and quantitatively over a long period of time.
[0166] More specifically, when the saturated moisture content is less than 1% by weight, it may be difficult to exhibit excellent sliding properties and the like.
[0167] On the other hand, when the saturated moisture content is a value exceeding 8% by weight, the dimensional change due to water absorption becomes large, and it may become difficult to maintain dimensional accuracy.
[0168] Therefore, the saturated moisture content is more preferably within a range of 1.5 to 7% by weight, and further preferably within a range of 2 to 6% by weight.
[0169] The saturated moisture content is measured in accordance with JIS K 7209:2000 and can be measured as a ratio of the increased weight due to absorbed moisture to the initial weight.
[0170] (8) Mixing amount
[0171] The amount of the uncarbonized carbon fibers as the compounding component (b) is preferably in the range of 10 to 400 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a).
[0172] The reason is that by regulating the amount of uncarbonized carbon fibers as the compounding component (b) to a value within a prescribed range, a sliding resin composition having a friction coefficient, wear amount and linear expansion coefficient below prescribed values can be more easily and stably provided when processed into a sliding part.
[0173] More specifically, if the blending amount of such uncarbonized carbon fibers is less than 10 parts by weight, it may be difficult to adjust the linear expansion coefficient to within a predetermined range when processed into sliding parts, or the wear resistance may decrease and the wear loss may increase.
[0174] On the other hand, if the amount of the uncarbonized carbon fiber blended is greater than 400 parts by weight, it may be difficult to adjust the friction coefficient value to within a specified range when the sliding resin composition is processed into a sliding part, or the molding processability when processed into a sliding part may be significantly reduced.
[0175] Therefore, the blending amount of the uncarbonized carbon fibers is more preferably within a range of 30 to 300 parts by weight, and even more preferably within a range of 50 to 200 parts by weight.
[0176] Here, refer to Figure 5 (a) The relationship between the blending amount of the uncarbonized carbon fibers and the linear expansion coefficient measured in accordance with JIS K 7197:2012 (hereinafter, sometimes simply referred to as the linear expansion coefficient) when processed into a sliding part is described.
[0177] Right now, Figure 5 The horizontal axis of (a) is the amount (parts by weight) of the uncarbonized carbon fiber relative to 100 parts by weight of the resin component (a), and the vertical axis is the linear expansion coefficient (1×10 -5 / ℃).
[0178] Moreover, as described later, Figure 5The characteristic curve in (a) is the linear expansion coefficient of the sliding parts of Examples 1, 4 to 7 and Comparative Examples 3 and 5, based on the values where the types of compounding components (a) to (c) and the compounding amount of compounding component (a) are the same and the compounding amount of compounding component (c) is in the range of 10 to 80 parts by weight.
[0179] According to the Figure 5 It can be understood from the characteristic curve described in (a) that the linear expansion coefficient tends to decrease as the blending amount of the uncarbonized carbon fibers increases.
[0180] More specifically, if the amount of the uncarbonized carbon fiber blended is less than 10 parts by weight, the linear expansion coefficient is greater than 5×10 -5 / ℃, but if it is 10 parts by weight or more, the linear expansion coefficient will be 5×10 -5 / ℃ or less.
[0181] Furthermore, if the amount of the uncarbonized carbon fibers blended exceeds 400 parts by weight, the linear expansion coefficient becomes 4×10 -5 / ℃ or below.
[0182] Therefore, it can be understood that by controlling the blending amount of the uncarbonized carbon fibers within a predetermined range, the value of the linear expansion coefficient in the sliding member can be adjusted with high accuracy.
[0183] Next, refer to Figure 5 (b) illustrates the relationship between the blending amount of uncarbonized carbon fibers and the friction coefficient when processed into sliding parts.
[0184] Right now, Figure 5 The horizontal axis of (b) represents the amount (parts by weight) of the uncarbonized carbon fiber relative to 100 parts by weight of the resin component (a), and the vertical axis represents the friction coefficient (-) obtained when the sliding component is processed according to Example 1 described later.
[0185] and, Figure 5 The characteristic curve in (b) is Figure 5 (a) Similarly, this is the result based on the friction coefficient of Examples 1, 4 to 7 and Comparative Examples 3 and 5.
[0186] From this Figure 5 It can be understood from the characteristic curve described in (b) that there is a tendency that the friction coefficient increases as the blending amount of the uncarbonized carbon fibers increases.
[0187] More specifically, when the blending amount of the uncarbonized carbon fibers exceeds 400 parts by weight, the friction coefficient becomes a value greater than 0.4, while when it is less than 400 parts by weight, particularly 10 to 200 parts by weight, a low value of 0.1 or less can be obtained.
[0188] Next, refer to Figure 5 (c) illustrates the relationship between the amount of uncarbonized carbon fibers added and the amount of wear when processed into sliding parts.
[0189] Right now, Figure 5 The horizontal axis of (c) is expressed by the amount of uncarbonized carbon fiber blended (parts by weight) relative to 100 parts by weight of the resin component (a), and the vertical axis is expressed by the wear amount (μm) under specified conditions when processed into a sliding part according to Example 1 described later.
[0190] and, Figure 5 The characteristic curve in (c) is Figure 5 (a) Similarly, this is the result based on the wear amount of Examples 1, 4 to 7 and Comparative Examples 3 and 5.
[0191] According to the Figure 5 It can be understood from the characteristic curve described in (c) that as the blending amount of the uncarbonized carbon fibers increases, the wear amount tends to decrease temporarily and then increase.
[0192] More specifically, when the blending amount of the uncarbonized carbon fiber is less than 10 parts by weight, the wear loss is greater than 100 μm, while when it is less than 400 parts by weight, particularly 10 to 200 parts by weight, a low value of 100 μm or less is obtained.
[0193] Therefore, by adjusting the amount of uncarbonized carbon fibers to a value within the range of 10 to 400 parts by weight, excellent sliding properties, i.e., low friction coefficient and small wear values, can be obtained while maintaining the linear expansion coefficient of the sliding part at a low level, thereby achieving a better balance between the two.
[0194] 3. Compounding ingredients (c)
[0195] (1) Types
[0196] It is preferred that a predetermined amount of an inorganic material is added as the compounding component (c), so that the mechanical strength, heat resistance, sliding properties, surface smoothness, etc. of the sliding part obtained by performing a predetermined process are improved.
[0197] More specifically, it is preferred that a predetermined amount of an inorganic material as the compounding component (c) is compounded to reduce the linear expansion coefficient and the like in the sliding member, thereby improving the sliding properties and the like.
[0198] Here, the type of the inorganic material as the blended component (c) is not particularly limited, but it is preferable to blend an inorganic material having a Mohs hardness of 6 or less.
[0199] More specifically, at least one of mica, talc, graphite, gypsum, kaolinite, zinc oxide, titanium oxide, zirconium oxide and the like is preferably added.
[0200] The reason for this is that these inorganic materials have a Mohs hardness of 6 or less and are low in hardness, so when they are made into sliding parts, the sliding resistance with the counterpart part can be reduced and the friction coefficient can be suppressed to a low level.
[0201] In addition, among these inorganic materials, if it is talc, mica, graphite, gypsum, kaolinite or a mixture thereof with a Mohs hardness of less than 4 (for example, the mixing weight ratio of talc / mica: 90 / 10 to 10 / 90), even a relatively small amount of the mixed amount can exhibit good sliding properties, etc., and therefore it can be said to be more suitable.
[0202] Furthermore, if the compounding component (c) is talc (hydrous magnesium silicate: Mg3Si4O 10 (OH)2 as the main component of the mineral) is relatively cheap and can be mixed evenly with the resin component as the compounding component (a), so it is preferred.
[0203] Furthermore, when talc or a mixture of talc and mica is used as the compounding component (c), the apparent density is relatively uniform and low.
[0204] More specifically, in the case of talc, the apparent density measured in accordance with JIS K 5101-12:2004 is preferably 0.1 to 0.8 g / ml, more preferably 0.2 to 0.7 g / ml, and still more preferably 0.3 to 0.6 g / ml.
[0205] Furthermore, these inorganic materials are more preferable because they can provide a smooth surface without hindering the predetermined fluidity even when the sliding parts are manufactured by injection molding, compression molding, or the like.
[0206] (2) Average particle size
[0207] The inorganic material as component (c) preferably has an average particle size measured in accordance with JIS Z8825:2013 (for example, D50 in particle size distribution obtained by laser diffraction, the same applies hereinafter) within a range of 1 to 180 μm.
[0208] The reason for this is that if the average particle size is less than 1 μm, the particles tend to aggregate, which not only makes handling difficult but also makes it difficult to uniformly mix with a resin component such as a PPS resin.
[0209] On the other hand, if the average particle size is larger than 180 μm, it may be difficult to obtain a smooth surface when manufacturing a sliding part by injection molding, compression molding, or the like.
[0210] Therefore, when an inorganic material such as talc is used as the compounding component (c), the average particle size is more preferably within a range of 10 to 110 μm, and further preferably within a range of 15 to 40 μm.
[0211] It should be noted that the influence of the above-mentioned average particle size becomes more significant as the amount of the inorganic material as the compounding component (c) increases relative to 100 parts by weight of the resin component as the compounding component (a).
[0212] (3) Mixing amount 1
[0213] The amount of the inorganic material as the compounding component (c) is usually within a range of 10 to 80 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a).
[0214] The reason for this is that if the amount of the compounded component (c) is less than 10 parts by weight, it may be difficult to adjust the linear expansion coefficient and the like within a predetermined numerical range when processing into a sliding part.
[0215] On the other hand, when the amount of the compounded component (c) is greater than 80 parts by weight, the melt viscosity of the sliding resin composition becomes high, and the molding processability when processing into a sliding part may be significantly reduced.
[0216] Therefore, the amount of the compounding component (c) is more preferably 15 to 60 parts by weight, and even more preferably 20 to 50 parts by weight, relative to 100 parts by weight of the resin component of the compounding component (a).
[0217] (4) Mixing amount 2
[0218] In addition, it is also preferred to determine the blending amount of the inorganic material as the blending component (c) in relation to the blending amount of the uncarbonized carbon fibers as the blending component (b).
[0219] More specifically, the weight ratio of the compounded component (b) / the compounded component (c) (hereinafter, sometimes simply referred to as the compounded amount ratio b / c) is preferably set to a value within the range of 1 / 1 to 10 / 1.
[0220] The reason for this is that by limiting the blending ratio b / c in the sliding resin composition, it is easier to adjust the linear expansion coefficient, friction coefficient and wear amount to values below predetermined values when processed into a sliding part.
[0221] More specifically, if the blending ratio b / c is a value smaller than 1 / 1, it may be difficult to adjust the linear expansion coefficient, wear amount, etc. within a predetermined numerical range when processing into a sliding part.
[0222] On the other hand, if the ratio b / c of the blending amount is larger than 10 / 1, it may be difficult to adjust the friction coefficient, wear amount, etc. within a predetermined numerical range when processing into a sliding part.
[0223] Therefore, the ratio b / c of the blending amount is more preferably a value within the range of 1.5 / 1 to 8 / 1, and further preferably a value within the range of 2 / 1 to 6 / 1.
[0224] Here, refer to Figure 6 (a) Regarding the amount of inorganic material mixed, the relationship between the ratio b / c of the amount mixed and the linear expansion coefficient is described.
[0225] Right now, Figure 6 The horizontal axis of (a) is the ratio of the compounding amount, i.e., compounding component (b) / compounding component (c) (-), and the vertical axis is the linear expansion coefficient (1×10 -5 / ℃).
[0226] Moreover, about Figure 6 The data of the characteristic curve of (a) are, as described later, the type and amount of the resin component as the compounding component (a) are the same, the types of the uncarbonized carbon fibers as the compounding component (b) and the inorganic material as the compounding component (c) are the same, based on the linear expansion coefficients of Examples 1, 4 to 7 and Comparative Examples 3 to 6.
[0227] According to the Figure 6 From the characteristic curve in (a), it can be seen that as the value of the ratio b / c of the compounding amount increases, the linear expansion coefficient decreases and tends to stabilize.
[0228] More specifically, when the ratio b / c of the blending amount is around 0 / 1, the linear expansion coefficient is 6×10 -5 / ℃, when the ratio b / c of the above-mentioned compounding amount is about 1 / 1, the linear expansion coefficient decreases sharply to 5×10 -5 / ℃ or below.
[0229] When the ratio b / c of the blending amount is about 10 / 1, the linear expansion coefficient is 4×10 -5 / ℃ value.
[0230] However, the ratio b / c of the blending amount further exceeds 10 / 1 and tends to decrease slightly until it reaches about 40 / 1, but is approximately 3.5×10 -5 ~4×10 -5 / ℃ range.
[0231] Therefore, when determining the amount of the inorganic material as the compounding component (c), when the compounding amount ratio b / c is, for example, a value within the range of 1 / 1 to 10 / 1, it can be said that the linear expansion coefficient of the sliding member can be accurately adjusted to a desired range.
[0232] In addition, refer to Figure 6 (b) Regarding the amount of inorganic material blended, the relationship between the blending ratio b / c and the friction coefficient when processed into a sliding part is described.
[0233] Right now, Figure 6 The horizontal axis of (b) shows the ratio of the blending amount, i.e., blending component (b) / blending component (c) (-), and the vertical axis shows the friction coefficient (-) obtained when the sliding part is processed according to Example 1 described later.
[0234] and, Figure 6 (b) The data of the characteristic curve and Figure 6 (a) Similarly, this is based on the friction coefficients of Examples 1, 4 to 7 and Comparative Examples 3 to 6.
[0235] According to the Figure 6 It can be understood from the characteristic curve in (b) that the friction coefficient tends to increase as the ratio b / c of the blending amount increases.
[0236] More specifically, when the ratio b / c of the blending amount is around 0 / 1, the friction coefficient is about 0.05. When the ratio b / c of the blending amount is around 1 / 1, there is some deviation depending on the conditions, but it is greater than 0.05. When it is around 10 / 1, it slowly increases to a value below 0.2.
[0237] In addition, refer to Figure 6 (c) Regarding the blending amount of the inorganic material, the relationship between the blending amount ratio b / c and the wear amount when processed into a sliding part is described.
[0238] Right now, Figure 6 The horizontal axis of (c) is expressed as the ratio of the blending amount, i.e., blending component (b) / blending component (c) (-), and the vertical axis is expressed as the wear amount (μm) under predetermined conditions when processed into a sliding part according to Example 1 described later.
[0239] and, Figure 6 (c) The data of the characteristic curve and Figure 6 (a) Similarly, this is based on the wear amount of Examples 1, 4 to 7 and Comparative Examples 3 to 6.
[0240] According to the Figure 6 From the characteristic curve in (c), it can be seen that as the ratio b / c of the blending amount increases, the wear amount tends to decrease temporarily and then increase.
[0241] More specifically, when the ratio b / c of the blending amount is around 0 / 1, the wear amount is about 150 μm, and when the ratio b / c of the blending amount is around 1 / 1, it decreases to less than 100 μm, and then increases to a value greater than 100 μm when it exceeds 10 / 1.
[0242] Therefore, according to this Figure 6 (a) to (c) It can be understood that by adjusting the ratio b / c of the compounding amount, excellent sliding properties, that is, low friction coefficient and small wear value can be obtained while maintaining the linear expansion coefficient in the sliding part at a low level, and the balance between the two can be further improved.
[0243] in addition, Figure 7 (a) and Figure 7 (b) is a cross-sectional photograph of a sliding member corresponding to Example 1 and Comparative Example 2 described later.
[0244] In this Figure 7 In (a), it can be understood that the sliding part is composed of a sliding resin composition 16, in which the carbon fibers 10 as specified uncarbonized carbon fibers are relatively uniformly dispersed not only in a specified direction but also in a direction orthogonal thereto, inside a resin component 12 containing an inorganic material 14.
[0245] On the other hand, Figure 7 In (b) as well, it was observed that the carbon fibers 10 were uniformly dispersed.
[0246] That is, from Figure 7 (a) and Figure 7 As can be understood from the cross-sectional photograph of (b), no difference due to the difference in the uniform dispersion of the carbon fibers 10 and the difference in the carbon amount due to the difference in the firing temperature of the carbon fibers 10 was observed, and the cross-sectional structures were in the same state.
[0247] Therefore, from these results, it can be said that even when predetermined uncarbonized carbon fibers are used, they can be uniformly dispersed, and low values of friction coefficient and wear amount can be obtained while maintaining the linear expansion coefficient of the sliding member at a low level.
[0248] 4. Compounding ingredients (d)
[0249] (1) Types
[0250] Furthermore, it is preferred to mix a lubricating additive which is different from the resin component of the mixed component (a) and which exhibits a lubricating effect as the mixed component (d).
[0251] The reason for this is that by adding such a lubricating additive, the lubricating property of the processed sliding part can be significantly improved by interacting with the components (a) to (c) constituting the sliding resin composition.
[0252] Furthermore, the type of the lubricating additive is not particularly limited as long as it is a compound that exerts a prescribed lubricating effect, and is preferably at least one of polytetrafluoroethylene (PTFE), perfluoroalkoxyalkane (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), perfluoroethylene-propylene copolymer (FEP), polyvinylidene fluoride (PVDF), silicone grease, silicone oil, silicone powder, and the like.
[0253] As the lubricating additive of the blending component (d), PTFE and ETFE, which are the above-mentioned fluororesins, are each preferred. PTFE is particularly preferred because it has a low friction coefficient, exhibits a lubricating effect, and can provide good wear resistance.
[0254] PTFE or the like is preferred because it can be uniformly mixed and dispersed with the PPS resin or the like as the resin component of the compounding component (a) even when compounded in a relatively wide range.
[0255] In addition, PTFE and the like are known to have various average particle sizes, and their average particle size (for example, D50 in the particle size distribution obtained by laser diffraction) is preferably a value in the range of 1 to 50 μm, more preferably a value in the range of 3 to 20 μm, and further preferably a value in the range of 5 to 10 μm.
[0256] (2) Quantity
[0257] The amount of the lubricating additive as the compounding component (d) is preferably generally within a range of 10 to 80 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a).
[0258] The reason for this is that if the amount of the compounded component (d) is less than 10 parts by weight, even if it is added to the sliding resin composition, the effect of addition such as imparting lubricity may not be exhibited.
[0259] On the other hand, if the amount of the compounded component (d) is greater than 80 parts by weight, it may be difficult to adjust the linear expansion coefficient of the processed lubricated member to a predetermined value or less.
[0260] Therefore, the amount of the compounding component (d) is more preferably 15 to 60 parts by weight, and even more preferably 20 to 40 parts by weight, relative to 100 parts by weight of the resin component as the compounding component (a).
[0261] 5. Other ingredients (e)
[0262] (1) Types
[0263] It is also preferred to mix, as the compounding component (e), compounds other than the above-mentioned compounding components (a) to (d), that is, various additives for achieving various purposes.
[0264] For example, as a friction property improver, it is preferred to mix at least one of modified polyolefin resins, mineral oils, ester oils, silicone oils and other lubricating oils, polyethylene waxes, oxidized polyethylene waxes, ester waxes, partially saponified waxes and other waxes, graphite, boron nitride, molybdenum disulfide, tungsten disulfide and other solid lubricants.
[0265] Even for oxidized polyethylene wax, if it is an oxidized polyethylene wax with a melting point of 120°C or above, it helps to maintain the mechanical strength and heat resistance of the sliding parts, and even if it is added in a relatively small amount, it helps to mix the various ingredients evenly, and it is easy to adjust the lubricity, moldability, etc., so it is preferred.
[0266] On the other hand, graphite is also a suitable compounding component (e), because lubricity, moldability, conductivity, hiding power, etc. can be easily adjusted by appropriately changing its compounding amount and form (average particle size, flaky shape).
[0267] (2) Quantity
[0268] When graphite or the like is added as the component (e), the amount thereof is preferably in a range of 1 to 50 parts by weight based on 100 parts by weight of the resin component as the component (a).
[0269] The reason for this is that, although it varies depending on the type of the compounded component (e), if the compounded amount is less than 1 part by weight, the compounding effect, particularly the effect of lubricity, may not be exhibited.
[0270] On the other hand, if the amount of the compounding component (e) is greater than 50 parts by weight, it may be difficult to uniformly mix the compounding component (a) with the resin component, or it may be difficult to adjust the lubricity, moldability, conductivity, hiding power, etc.
[0271] Therefore, the amount of the compounding component (e) is more preferably 1.5 to 30 parts by weight, and even more preferably 2 to 10 parts by weight, relative to 100 parts by weight of the resin component as the compounding component (a).
[0272] 6. Manufacturing method
[0273] The sliding resin composition of the present invention is preferably prepared by mixing using a mixer such as a Henschel mixer, a super mixer, a ball mill or a tumble mixer while weighing the various ingredients in the composition so that the amounts thereof fall within a predetermined range.
[0274] Next, when the resin component (a) of the sliding resin composition is a thermoplastic resin, the mixture is preferably fed into a vented single-shaft or twin-shaft screw extruder or a non-vented single-shaft or twin-shaft screw extruder, melt-kneaded to form a strip-shaped molding, and then the molding is cut into granular molding material pellets.
[0275] By making such molding material pellets, in the method for manufacturing a sliding component described later, the pellets can be molded into a desired shape such as a cylindrical bushing or a plate-like body by molding means such as an injection molding device.
[0276] When the resin component (a) of the sliding resin composition is a thermosetting resin, after the mixture is prepared by the mixer, it is preferably placed in a mold in the state of the mixture for compression molding.
[0277] Thus, the sliding resin composition put into the mold can be cured by applying heat and pressure in a heating press for a predetermined time, and after compression molding, it can be dried in a drying furnace for a predetermined time to allow the curing reaction to proceed sufficiently, thereby obtaining a desired sliding component.
[0278] [Second embodiment]
[0279] The second embodiment is a sliding member characterized in that the linear expansion coefficient measured in accordance with JIS K 7197:2012 is 5×10 -5 The sliding component having a temperature of 1000 W / °C or less is derived from a sliding resin composition containing the following compounding components (a) to (c).
[0280] (a) Resin component: 100 parts by weight
[0281] (b) 5 wt% uncarbonized carbon fibers with a reduction temperature of 400 to 550°C: 10 to 400 parts by weight
[0282] (c) Inorganic materials: 10 to 80 parts by weight
[0283] 1. Basic structure
[0284] A submersible pump can be taken as an example of a mechanical device or the like using the sliding member of the present invention, and basically any submersible pump having any structure is applicable as long as it uses a sliding member such as a sliding bearing.
[0285] Therefore, for example, any submersible pump that has 1) an impeller, 2) a shaft for fixing the impeller, 3) a sliding bearing fixed to the impeller and used to support the impeller so that it can rotate freely relative to the shaft, 4) a thrust bearing component that slides with each end surface of the sliding bearing, and 5) a casing and a cover that accommodate the impeller and constitute a pump chamber can be appropriately applied.
[0286] 2. Sliding parts
[0287] (1) Sliding resin composition
[0288] The sliding resin composition used in the sliding member of the second embodiment may be the same as that described in the first embodiment.
[0289] Therefore, the re-explanation of the sliding resin composition will be omitted here.
[0290] (2) Sliding parts made from sliding resin compositions
[0291] The basic structure of the sliding component obtained by including uncarbonized carbon fibers and treating the sliding resin composition is not particularly limited, and various modifications may be made.
[0292] That is, at least one or sometimes multiple sliding bearings are provided as sliding parts of the submersible pump, but as a basic structure, a cylindrical bearing or a flanged bearing having the same thickness as the end surface and bearing loads on the inner diameter and end surface is preferred.
[0293] Furthermore, since the resin composition for sliding use using a linear polyphenylene sulfide resin as a base resin can exhibit toughness in addition to having extremely low water absorption, it is preferably an injection-molded article.
[0294] 3. Manufacturing method
[0295] The method for producing a sliding member from the sliding resin composition is not particularly limited, but typically, an injection molding method or a compression molding method is preferably used.
[0296] (1) Injection molding
[0297] That is, according to the injection molding method, although it is just an example, a predetermined sliding member can be manufactured through the following steps 1) to 5).
[0298] 1) Prepare the injection molding device.
[0299] 2) The sliding resin composition as molding material pellets is weighed and placed in a hopper or the like of an injection molding device.
[0300] 3) The sliding resin composition is molten by a heating device of an injection molding device.
[0301] 4) Using an injection molding device, the molten sliding resin composition is injected into a predetermined mold.
[0302] 5) After cooling, take out the specified sliding parts.
[0303] (2) Compression molding
[0304] The compression molding method is also an example, but a predetermined sliding member can be manufactured through the following steps 1') to 4').
[0305] 1′) Prepare a predetermined molding die.
[0306] 2') The sliding resin composition, which is a mixture mixed in a mixer, is placed in a predetermined location of a molding die.
[0307] 3') Apply heat and pressure with a heated press for a certain period of time to cure it.
[0308] 4′) After compression molding, the predetermined sliding parts are taken out after drying in a drying furnace for a predetermined time.
[0309] 4. Characteristic 1 (Linear Expansion Coefficient)
[0310] The linear expansion coefficient of the sliding member can be measured using a thermomechanical analyzer (TMA) in accordance with JIS K 7197:2012 under the following prescribed conditions.
[0311] That is, a square test piece with a thickness of 3 mm and a single length of 5 mm was produced by molding, and the temperature of the square test piece was raised from 25°C to 100°C at 5°C / min using TMA. The change in the length of the square test piece was measured, and the linear expansion coefficient of the resin in the thickness direction (MD) at 35 to 80°C was calculated as the linear expansion coefficient.
[0312] In addition, it is generally preferred that the linear expansion coefficient be 5×10 -5 / ℃ below.
[0313] The reason is that if the linear expansion coefficient is greater than 5×10 -5 / °C, the desired dimensional accuracy may not be maintained due to sliding heat, and the sliding properties and durability of the sliding parts may be significantly reduced.
[0314] However, if the linear expansion coefficient becomes too small, the types, forms, and blending amounts of selectable resin components, inorganic materials, uncarbonized carbon fibers, and the like may be excessively limited.
[0315] Therefore, the linear expansion coefficient of the sliding member is more preferably 1×10 -5 / ℃~4.8×10-5 / °C, more preferably 2×10 -5 / ℃~4.6×10 -5 / ℃ range.
[0316] Here again, refer to Figure 1 (a) The relationship between the sintering temperature of carbon fibers (including uncarbonized carbon fibers and other carbon fibers) and the linear expansion coefficient when processed into a sliding member including the carbon fibers is described.
[0317] Right now, Figure 1 The horizontal axis of (a) represents the calcination temperature of the carbon fiber (°C), and the vertical axis represents the linear expansion coefficient (1×10 -5 / ℃) relationship.
[0318] Moreover, as described later, Figure 1 The data of the characteristic curve (a) are based on the linear expansion coefficients of Examples 1 to 3 and Comparative Examples 1 and 2, in which the types and amounts of the compounding components (a) to (c) are the same and only the sintering temperatures of the carbon fibers are different.
[0319] According to the Figure 1 It can be understood from the characteristic curve described in (a) that the firing temperature (°C) of the carbon fibers has no significant influence on the linear expansion coefficient of the sliding member.
[0320] 5. Characteristic 2 (friction coefficient)
[0321] The friction coefficient of the sliding member can be measured under the following conditions using a thrust unidirectional rotation method in accordance with JIS K 7218:1986.
[0322] Sliding speed: 90m / min
[0323] Load (surface pressure): 10kg / cm 2
[0324] Test time: 20 hours
[0325] Test piece: Rectangular plate of 30 mm (horizontal width) × 30 mm (vertical width) × 3 mm (thickness)
[0326] Target material: Hollow cylindrical (SUS 304, inner diameter 20mm, outer diameter 25.6mm, length 15mm, surface roughness Ra 0.1)
[0327] Lubrication conditions: No lubrication
[0328] Furthermore, it is usually preferred that the friction coefficient be a value of 0.4 or less.
[0329] The reason for this is that if the friction coefficient exceeds 0.4, the sliding properties and durability of the sliding member may be significantly reduced.
[0330] Although it varies depending on the purpose and form of the sliding member, the friction coefficient is more preferably a value within the range of 0.01 to 0.2, and even more preferably a value within the range of 0.03 to 0.1.
[0331] in addition, Figure 1 (b) is a diagram for explaining the relationship between the calcination temperature of carbon fibers (including uncarbonized carbon fibers and carbon fibers other than carbon fibers) and the friction coefficient when processed into a sliding part including the carbon fibers.
[0332] Right now, Figure 1 The horizontal axis of (b) represents the calcination temperature (°C) of the carbon fibers, and the vertical axis represents the friction coefficient (-) obtained when a sliding resin composition prepared by blending carbon fibers calcined at a predetermined temperature is processed into a sliding part.
[0333] Moreover, as described later, Figure 1 The data of the characteristic curve (b) are based on the friction coefficient of Examples 1 to 3 and Comparative Examples 1 and 2, in which the types and amounts of the compounding components (a) to (c) are the same and only the sintering temperature of the carbon fiber is different.
[0334] By this Figure 1 From the characteristic curve (b), it can be seen that the lower the sintering temperature of the carbon fiber is, the more the friction coefficient in the sliding part tends to decrease.
[0335] More specifically, it can be understood that when the carbon fiber is fired at about 1250°C, the friction coefficient of the sliding component can be adjusted to a value below 0.4, and when the carbon fiber is fired at about 800°C, the friction coefficient can be adjusted to a value of about 0.1.
[0336] 6. Characteristic 3 (Durability)
[0337] In addition, the endurance time which is a standard of the sliding property of the sliding member can be measured using the above-mentioned thrust unidirectional rotation method.
[0338] Furthermore, generally, as a criterion for good sliding properties, the durability time of the sliding member is preferably 10 hours or more.
[0339] Although it varies depending on the purpose, form, etc. of the sliding component, the durability time is more preferably 15 hours or more, and further preferably 20 hours or more.
[0340] 7. Characteristic 4 (wear amount)
[0341] The wear amount, which is another criterion of the sliding property of the sliding member, can be measured under the same conditions using the above-mentioned thrust one-way rotation method.
[0342] That is, the thrust unidirectional rotation method was performed for a predetermined time (20 hours), and the thickness change of the test piece composed of the sliding member from the initial value after the lapse of 20 hours was calculated as the wear amount.
[0343] Furthermore, generally, as a criterion for good sliding properties, the wear amount of the test piece is preferably 100 μm or less.
[0344] Although it varies depending on the purpose, form, etc. of the sliding member, the wear amount of the test piece is more preferably 80 μm or less, and further preferably 50 μm or less.
[0345] If melting was observed on the test piece before 20 hours had passed, the test by the thrust unidirectional rotation method was terminated at that time, and the thickness change from the initial value of the test piece composed of the sliding member was calculated as the wear amount.
[0346] in addition, Figure 1 (c) is a graph for explaining the relationship between the sintering temperature of carbon fibers (including uncarbonized carbon fibers and other carbon fibers) and the wear amount under the above-mentioned predetermined conditions when processed into a sliding part including the carbon fibers.
[0347] Right now, Figure 1 The horizontal axis of (c) represents the calcination temperature (°C) of the carbon fibers, and the vertical axis represents the relationship between the wear loss (μm) under the above measurement conditions when a sliding resin composition prepared by mixing carbon fibers calcined at a predetermined temperature is processed into a sliding part.
[0348] Moreover, as described later, Figure 1 The data of the characteristic curve (c) are based on the wear amount of Examples 1 to 3 and Comparative Examples 1 and 2, in which the types and amounts of the compounding components (a) to (c) are the same and only the sintering temperature of the carbon fiber is different.
[0349] It should be noted that according to the Figure 1 It can be understood from the characteristic curve (c) that as the sintering temperature of the carbon fiber increases, the wear amount tends to decrease temporarily and then increase.
[0350] More specifically, when the sintering temperature of the carbon fiber is lower than 600°C, the wear amount becomes a value larger than 100 μm, but becomes 100 μm or less at 600°C, and becomes a value larger than 100 μm again when the temperature exceeds 800°C.
[0351] Therefore, if we consider Figure 1From the results of the characteristic curves shown in (a) to (c), it can be said that by adjusting the sintering temperature of the carbon fiber to a specified range (below 800°C, especially 600 to 800°C), a good balance between the linear expansion coefficient and the sliding properties can be achieved when processed into sliding parts, and the linear expansion coefficient can be maintained at a low level and the friction coefficient and wear amount as sliding properties can be controlled below the specified values.
[0352] [Example]
[0353] Hereinafter, the present invention will be described in detail based on examples, but the scope of rights of the present invention will not be narrowed by the description of the examples unless there is a particular reason.
[0354] In addition, the resin as the compounding component (a), the uncarbonized carbon fiber as the compounding component (b), the inorganic material as the compounding component (c), and the lubricating additive as the compounding component (d) used in the examples are as follows.
[0355] (A) Compounding ingredients (a)
[0356] (A-1) Polyphenylene sulfide resin (PPS resin) (manufactured by Polyplastics Co., Ltd., trade name “DURAFIDE”, type of PPS resin: linear type)
[0357] (A-2) Polyetheretherketone resin (PEEK resin) (manufactured by Solvay Specialty Polymers Co., Ltd., trade name "KETASPIRE")
[0358] (A-3) Polyethersulfone resin (PES resin) (manufactured by Sumitomo Chemical Co., Ltd., trade name "SUMIKAEXCEL"
[0359] (B) Compounding ingredients (b)
[0360] (B-1) Isotropic pitch-based uncarbonized carbon fiber 1 (sintering temperature: 700° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 5.8 wt %)
[0361] (B-2) Isotropic pitch-based uncarbonized carbon fibers 2 (sintering temperature: 650° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 5.5 wt %)
[0362] (B-3) Isotropic pitch-based uncarbonized carbon fibers 3 (sintering temperature: 750° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 6.5 wt %)
[0363] (B') corresponds to carbon fiber of compounding component (b)
[0364] (B′-1) Isotropic pitch-based carbon fiber 1 (sintering temperature: 450° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 8.5 wt %)
[0365] (B′-2) Isotropic pitch-based carbon fiber 2 (sintering temperature: 1300° C., sintering time: 30 minutes, average diameter: 15 μm, average length: 200 μm, saturated moisture content: 0.5 wt %)
[0366] (C) Compounding ingredients (c)
[0367] (C-1) Talc (manufactured by Nippon Talc Co., Ltd., trade name "MS-P", average particle size: 14 μm)
[0368] (C-2) Mica (manufactured by Yamaguchi Mica Co., Ltd., trade name "J-31M", average particle size: 23 μm)
[0369] (D) Compounding ingredients (d)
[0370] (D-1) Polytetrafluoroethylene (PTFE) (manufactured by AGC Corporation, trade name “FLUON (registered trademark) PTFE”, average particle size: 5 μm)
[0371] (D-2) Perfluoroalkoxyalkane (PFA) (manufactured by Daikin Industries, Ltd., trade name “NEOFLON”, average particle size: 5 μm)
[0372] [Example 1]
[0373] 1. Preparation of sliding resin composition and evaluation parts
[0374] (1) Preparation of sliding resin composition
[0375] As shown in Table 1, in a specified container with a stirrer, 100 parts by weight of PPS resin A-1 as the resin component of the compounding component (a), 100 parts by weight of B-1 as the uncarbonized carbon fiber as the compounding component (b), and 30 parts by weight of the inorganic material C-1 as the compounding component (c) are weighed and accommodated.
[0376] As shown in Table 2, it was confirmed by TGA that TG5 was 450°C only for the uncarbonized carbon fibers of the blended component (b).
[0377] Furthermore, the amount of carbon on the surface of the uncarbonized carbon fibers of the blended component (b) was separately confirmed to be 93% by weight by XPS elemental analysis.
[0378] Next, a 20-L mixer was used as a stirrer to stir the components (a) to (c) at a rotation speed of 400 rpm for 90 seconds so that the components (a) to (c) were uniformly blended to prepare a sliding resin composition.
[0379] Next, the obtained sliding resin composition was dried using a heating furnace heated to 130° C. in the air to prepare a sliding resin composition (in powder form) having a water content of 0.01% by weight or less.
[0380] Next, the obtained sliding resin composition (powdered form) was melt-kneaded using a twin-screw extruder to prepare a pelletized composition.
[0381] (2) Preparation of evaluation parts
[0382] After the obtained sliding resin composition (pellet form) is filled into a specified mold using an injection molding device, the evaluation component A, which is press-molded into a plate-shaped evaluation component of 5 mm (lateral width) × 5 mm (vertical width) × 3 mm (thickness), and the evaluation component B, which is press-molded into a plate-shaped evaluation component of 30 mm (lateral width) × 30 mm (vertical width) × 3 mm (thickness), are obtained under specified pressurizing conditions (for example, 10 to 200 MPa).
[0383] The evaluation parts are substitute parts for evaluating various properties of sliding parts obtained by processing the sliding resin composition. Among the evaluation parts, the evaluation part A is used in the evaluation 6 (linear expansion coefficient) described later, and the evaluation part B is used in the evaluation 7 (friction coefficient), evaluation 8 (durability time) and evaluation 9 (wear amount) described later.
[0384] 2. Evaluation of sliding resin composition and sliding parts
[0385] (1) Evaluation 1 (firing temperature)
[0386] The calcination temperature of the carbon fibers was evaluated according to the following evaluation criteria. The results are shown in Table 2.
[0387] ◎: Temperature of 650 to 750°C.
[0388] 0: A temperature of 600 to less than 650°C or a temperature of more than 750 to 800°C.
[0389] △: A temperature of 500 to less than 600°C or a temperature of 800 to 1000°C.
[0390] ×: Temperature lower than 500°C or temperature higher than 1000°C.
[0391] (2) Evaluation 2 (tensile elastic modulus)
[0392] The tensile modulus of carbon fiber was measured in accordance with JIS R7606:2000 and evaluated according to the following evaluation criteria.
[0393] ◎:15~25GPa.
[0394] 0: less than 10-15 GPa or greater than 25-35 GPa.
[0395] △: less than 1~10GPa or greater than 35~50GPa.
[0396] ×: less than 1 GPa or greater than 50 GPa.
[0397] (3) Evaluation 3 (tensile elongation)
[0398] The tensile elongation of carbon fibers was measured in accordance with JIS R7606:2000 and evaluated according to the following evaluation criteria.
[0399] ◎:2.3~4%.
[0400] ○: less than 2-2.3% or greater than 4-5%.
[0401] △: 1.5 to less than 2% or greater than 5 to 6%.
[0402] ×: less than 1.5% or more than 6%.
[0403] (4) Evaluation 4 (Volume Resistivity)
[0404] The volume resistivity of the carbon fibers was measured by a four-terminal method using a digital voltmeter, and evaluated according to the following evaluation criteria.
[0405] ◎:5×10 0 ~1×10 3 Ω·cm.
[0406] 0:1×10 0 ~5×10 0 Ω·cm or greater than 1×10 3 ~1×10 4 Ω·cm.
[0407] △: 1×10 -1 ~1×10 0 Ω·cm or greater than 1×10 4 ~1×10 5 Ω·cm.
[0408] ×: less than 1×10 -1 Ω·cm or greater than 1×10 5 Ω·cm.
[0409] (5) Rating 5 (TG5)
[0410] The TG5 (5 wt% reduction temperature) of the carbon fiber was measured using TGA (manufactured by Mettler-Toledo, product name "TGA / SDTA851e") at an air flow rate of 100 ml / min and a heating rate of 5°C / min, and the evaluation was performed according to the following evaluation criteria. The results are shown in Table 2.
[0411] ◎:430~500℃.
[0412] 0: 400 to less than 430°C or 500 to 550°C.
[0413] △: 350~less than 400℃ or 550~600℃.
[0414] ×: less than 350°C or more than 600°C.
[0415] (6) Evaluation 6 (Linear Expansion Coefficient)
[0416] The linear expansion coefficient of the resin molded product as the sliding part was measured using the evaluation member A in accordance with JIS K 7197:2012 using a thermomechanical analyzer (manufactured by Mettler-Toledo, product name “TMA / SDTA841e”) and evaluated according to the following evaluation criteria.
[0417] ◎:4.5×10 -5 / ℃ below.
[0418] 0: 5×10 -5 / ℃ below.
[0419] △: 5.5×10 -5 / ℃ below.
[0420] ×: greater than 5.5×10 -5 / ℃.
[0421] (7) Evaluation 7 (friction coefficient)
[0422] The friction coefficient, which is one of the criteria for the sliding properties of sliding parts, was measured using the thrust unidirectional rotation method described above under the above-described prescribed conditions in accordance with JIS K 7218:1986 using the evaluation part B as the object, and then evaluated according to the following evaluation criteria.
[0423] ◎: 0.05 or less.
[0424] 〇: 0.1 or less.
[0425] △: 0.4 or less.
[0426] ×: greater than 0.4.
[0427] (8) Rating 8 (Durability)
[0428] Regarding the durability time, which is one of the criteria for the sliding properties of sliding parts, the time until the melting phenomenon occurred was measured using the thrust unidirectional rotation method described above in accordance with JIS K 7218:1986 using the evaluation part B as the object, and the evaluation was performed according to the following evaluation criteria.
[0429] ◎: No melting phenomenon was observed within 20 hours.
[0430] ○: No melting phenomenon was observed for more than 10 hours.
[0431] △: No melting phenomenon was observed for more than 1 hour.
[0432] ×: Melting phenomenon was observed in less than 1 hour.
[0433] (9) Evaluation 9 (wear loss)
[0434] The evaluation member B was used as an object, and the wear amount, which is one of the criteria for sliding properties of sliding members, was measured after 20 hours using the thrust unidirectional rotation method according to JIS K 7218:1986, and the wear amount was evaluated according to the following evaluation criteria.
[0435] If melting was observed in the evaluation member before 20 hours had passed, the test by the thrust unidirectional rotation method was terminated at that time, and the thickness change from the initial value of the evaluation member was calculated as the wear amount.
[0436] ◎: 50 μm or less.
[0437] 0: 80 μm or less.
[0438] △: 100 μm or less.
[0439] ×: larger than 100 μm.
[0440] [Examples 2-3]
[0441] In Examples 2 and 3, except that B-2 and B-3 were used as the uncarbonized carbon fibers of the compounding component (b), respectively, the sliding resin compositions and evaluation parts were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0442] As shown in Table 2, TG5 was separately confirmed to be 440° C. and 460° C. by TGA only for the uncarbonized carbon fibers as the blending component (b).
[0443] Furthermore, the carbon amounts on the surfaces of the uncarbonized carbon fibers as the blending component (b) were separately confirmed to be 90 wt % and 95 wt % by XPS elemental analysis.
[0444] [Examples 4 to 5]
[0445] In Examples 4 and 5, the amount of uncarbonized carbon fiber as the compounding component (b) was changed to 50 parts by weight and 120 parts by weight, respectively, relative to 100 parts by weight of the resin component as the compounding component (a). In addition, the sliding resin composition and the evaluation component were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0446] [Examples 6 to 7]
[0447] In Examples 6 and 7, the amount of the inorganic material as the compounding component (c) was changed to 60 parts by weight and 80 parts by weight, respectively, relative to 100 parts by weight of the resin component as the compounding component (a). The sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0448] [Examples 8 to 9]
[0449] In Examples 8 and 9, except that the type of the resin component as the formulation component (a) was changed to A-2 and A-3, respectively, the sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0450] [Examples 10-11]
[0451] In Examples 10 and 11, except that the type of the inorganic material as the compounding component (c) was changed to C-2 and a mixture of C-1 / C-2 (mixing weight ratio: 80 / 20), the sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0452] [Examples 12-13]
[0453] In Examples 12 and 13, except that the type (D-1, D-2) and the amount (5 parts by weight, 25 parts by weight) of the lubricating additive as the compounding component (d) were changed and added respectively, the sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0454] [Comparative Examples 1-2]
[0455] In Comparative Examples 1 and 2, except that the carbon fibers corresponding to the compounding component (b) were changed to B'-1 and B'-2, respectively, the sliding resin compositions and evaluation parts were prepared in the same manner as in Example 1, and each evaluation was performed. The evaluation results obtained are shown in Tables 1 and 2.
[0456] As shown in Table 2, only the carbon fibers corresponding to the blended component (b) were separately confirmed to have TG5 of 390° C. and 560° C. using TGA.
[0457] Furthermore, the amounts of carbon on the surface of the carbon fibers corresponding to the blended component (b) were separately confirmed to be 84% by weight and 97% by weight according to XPS elemental analysis.
[0458] [Comparative Example 3]
[0459] In Comparative Example 3, the amount of uncarbonized carbon fiber as the compounding component (b) was changed to 0.5 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a). The sliding resin composition and the evaluation component were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0460] [Comparative Example 4]
[0461] In Comparative Example 4, the amount of the inorganic material as the compounding component (c) was changed to 5 parts by weight relative to 100 parts by weight of the resin component as the compounding component (a). The sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0462] [Comparative Example 5]
[0463] In Comparative Example 5, the amount of uncarbonized carbon fiber as the compounding component (b) was changed to 450 parts by weight, and the amount of inorganic material as the compounding component (c) was changed to 10 parts by weight, respectively, relative to 100 parts by weight of the resin component as the compounding component (a). The sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0464] [Comparative Example 6]
[0465] In Comparative Example 6, the amount of uncarbonized carbon fiber as the compounding component (b) was changed to 50 parts by weight, and the amount of inorganic material as the compounding component (c) was changed to 100 parts by weight, respectively, relative to 100 parts by weight of the resin component as the compounding component (a), and the sliding resin composition and the evaluation member were prepared in the same manner as in Example 1, and each evaluation was performed. The obtained evaluation results are shown in Tables 1 and 2.
[0466]
[0467]
[0468] [Industrial Availability]
[0469] As described above, according to the sliding resin composition of the present invention, by containing the compounding component (b) which is a predetermined uncarbonized carbon fiber together with the inorganic material as the compounding component (c) for at least the resin component as the compounding component (a), when processed into a sliding part, a good balance between sliding properties and linear expansion coefficient can be obtained, and the friction coefficient and wear amount as sliding properties and the linear expansion coefficient can be maintained at low values.
[0470] That is, according to the present invention, it is possible to provide a sliding resin composition that can achieve excellent sliding properties and a low linear expansion coefficient for a long period of time, and a sliding part made from such a sliding resin composition.
[0471] More specifically, even for a member whose counterpart material is stainless steel (eg, Vickers hardness: 150 HV or more), the friction coefficient is low and the amount of wear can be reduced over a long period of time.
[0472] Therefore, the sliding resin composition of the present invention can be used as a machine part having excellent low friction and wear resistance, for example, in various bearings, by means of predetermined processing.
[0473] That is, it is expected to be widely used as a sliding part of a submersible pump or other liquid pump for circulating cooling water, chemical liquid, solvent, oil, beverage, etc. for automobile engines, inverters, batteries or fuel cells, and circulating hot water for water heaters, floor heating equipment, etc.
[0474] For example, in the case of bearings for submersible pumps, if there is sufficient water on the sliding surface, it will be close to a fluid lubrication state and good sliding properties can be obtained. However, in the early stage of pump operation, the bearing and the counterpart shaft will rub in a dry state, so good sliding properties are required even under dry conditions.
[0475] Furthermore, it is necessary to maintain dimensional accuracy so that the clearance fluctuation due to thermal expansion does not cause play in a predetermined device, the influence of locking on a mating axis, or the influence of sliding properties in water lubrication, and thus a small linear expansion coefficient is required.
[0476] In this regard, the sliding bearing of the water pump in the prior art Patent Document 1 contains at least one of polytetrafluoroethylene resin and graphite as a lubricant, but the sliding property is not sufficient to obtain the sliding property. That is, if the proportion of the lubricant is increased in order to obtain good low friction even under dry conditions, the linear expansion coefficient will increase significantly, and the strength of the bearing itself will decrease, which will deteriorate the wear resistance.
[0477] On the other hand, if the proportion of carbon fiber is increased in order to suppress the linear expansion coefficient to a low level and improve the wear resistance, low friction cannot be achieved, and the object material may be damaged.
[0478] However, with the sliding component made from the sliding resin composition of the present invention, even when the blending ratio of the carbon fiber is relatively reduced, the above-mentioned problems peculiar to the submersible pump bearing can be effectively suppressed.
[0479] Therefore, the sliding resin composition of the present invention and the sliding parts made from such a sliding resin composition are suitable for a wide range of uses, and are particularly suitable for use in bearings for submersible pumps.
Claims
1. A sliding resin composition, characterized in that Contains the following ingredients (a) to (c): (a) resin component: 100 parts by weight; (b) 5 wt% uncarbonized carbon fibers having a reduction temperature of 400 to 550°C: 10 to 400 parts by weight; (c) Inorganic material: 10 to 80 parts by weight.
2. The sliding resin composition according to claim 1, characterized in that The tensile modulus of the compounding component (b) measured in accordance with JIS R7606:2000 is a value within the range of 10 to 35 GPa.
3. The sliding resin composition according to claim 1 or 2, characterized in that The tensile elongation of the compounding component (b) measured in accordance with JIS R7606:2000 is a value within the range of 2 to 5%.
4. The sliding resin composition according to any one of claims 1 to 3, characterized in that The amount of carbon on the surface of the blending component (b) as determined by XPS elemental analysis is within a range of 85 to 96% by weight relative to the total amount.
5. The sliding resin composition according to any one of claims 1 to 4, characterized in that When processed into sliding parts, the linear expansion coefficient measured in accordance with JIS K7197:2012 is 5×10 -5 / ℃ below.
6. The sliding resin composition according to any one of claims 1 to 5, characterized in that The weight ratio of the compounding component (b) to the compounding component (c) is a value within a range of 1 / 1 to 10 / 1.
7. The sliding resin composition according to any one of claims 1 to 6, characterized in that The compounding component (a) is at least one selected from polyphenylene sulfide resin, polyethersulfone resin, polyetheretherketone resin, polyimide resin and thermosetting phenolic resin.
8. A sliding component, characterized in that: The linear expansion coefficient measured according to JIS K7197:2012 is 5×10 -5 / °C or less, and is derived from a sliding resin composition containing the following blending components (a) to (c): (a) resin component: 100 parts by weight; (b) 5 wt% uncarbonized carbon fibers having a reduction temperature of 400 to 550°C: 10 to 400 parts by weight; (c) Inorganic material: 10 to 80 parts by weight.