Composition for temporary fixing
By using a specific combination of temporary fixatives in electronic device manufacturing, the bubble problem and high-temperature processing requirements in the spin coating process are solved, achieving efficient bubble reduction and rapid peeling effects.
Patent Information
- Application Number
- CN202380024634.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-01-19
- Publication Date
- 2024-10-15
AI Technical Summary
In the manufacturing process of electronic equipment, existing temporary fixatives are prone to generate bubbles during the spin coating process, causing adverse effects on physical properties, and are difficult to meet the needs of high-temperature processing and rapid peeling.
A composition containing monofunctional (meth)acrylate, multifunctional (meth)acrylate and photoradical polymerization initiator is used to form a temporary fixing agent with suitable viscosity and surface properties by adjusting its viscosity and surface tension, thereby reducing Air bubbles are mixed in and remain stable at high temperatures.
It effectively reduces the mixing of bubbles in the spin coating process, improves the heat resistance of high-temperature processing and the speed of laser peeling, and ensures the flatness and easy peeling of the substrate.
Smart Images

Figure BDA0005019583170000201 
Figure BDA0005019583170000211 
Figure BDA0005019583170000221
Abstract
Description
Technical Field
[0001] The present invention relates to a composition for temporary fixing. Background Art
[0002] When manufacturing electronic devices, wafer-type substrates with a thickness of about several hundred μm are often used. These are obtained by using an inorganic material represented by silicon as a substrate and performing processes such as insulating film formation, circuit formation, and thinning by grinding on its surface. However, most substrates are made of brittle materials and easily break, so measures are required to prevent damage, especially when thinning by grinding. Regarding this measure, a method has been adopted so far of attaching a temporary fixing protective tape that can be peeled off after the processing step is completed to the surface opposite to the grinding object (also called the back side). This tape uses an organic resin film as a base material and has flexibility, but lacks strength or heat resistance and is not suitable for use in high-temperature processes.
[0003] Therefore, a system has been proposed that provides sufficient durability to withstand the conditions of back-side grinding and back-side electrode formation processes by bonding electronic device substrates to a support such as silicon or glass via an adhesive. The adhesive layer used to bond the substrate to the support is crucial. This adhesive layer must ensure a seamless bond between the substrate and the support, possess sufficient durability to withstand subsequent steps, and ultimately allow for easy separation of the thinned wafer from the support; in other words, it must provide temporary fixation.
[0004] The main steps in processing such a wafer include spin coating, vacuum bonding and photocuring, thinning by grinding and polishing, high-temperature treatment, laser lift-off, and temporary bonding agent removal.
[0005] In order to uniformly form a film of the temporary fixing agent on the wafer during the spin coating process, the temporary fixing agent is required to have an appropriate viscosity and be a Newtonian fluid (or have a shear viscosity that is independent of shear rate).
[0006] In the vacuum bonding / UV curing process, the temporary bonding agent is required to be cured in a short time by irradiation with ultraviolet (UV) light or the like on a support such as glass, and to generate little outgassing (low outgassing properties).
[0007] To prevent damage caused by localized load from the grinder applied to the substrate during thinning processes such as grinding and polishing, the temporary fixative must have moderate hardness to distribute the load in-plane and prevent localized substrate sinking, thereby maintaining planarity. Furthermore, it must have strong adhesion to the support, a moderately high elastic modulus to protect the edges, and chemical resistance.
[0008] In the high-temperature treatment process, the temporary bonding agent needs to have heat resistance that can withstand high-temperature treatment in a vacuum for a long period of time (for example, at a temperature of 300° C. or higher for more than one hour).
[0009] In the laser lift-off process, the temporary bonding agent needs to be able to be removed at high speed by a laser such as a UV laser.
[0010] In the removal process, in addition to easy peelability for easily peeling the substrate from the support, cohesive properties for preventing adhesive residue from remaining on the substrate after peeling and easy cleaning are also required.
[0011] In view of this background, for example, Patent Document 1 discloses a temporary fixing composition comprising: (A-1) a monofunctional (meth)acrylate having an alkyl group with 18 or more carbon atoms as a side chain and a homopolymer having a Tg of -100°C to 60°C; (A-2) a polyfunctional (meth)acrylate; (B) a polyisobutylene monomer and / or a polyisobutylene copolymer; and (C) a photoradical polymerization initiator. This temporary fixing composition is said to have excellent heat resistance, low outgassing properties, and releasability.
[0012] Prior art literature
[0013] Patent Literature
[0014] Patent Document 1: International Publication No. 2021 / 235406 Summary of the Invention
[0015] When a conventional temporary bonding agent is applied to a wafer by spin coating, there have been reports of bubbles being generated in the temporary bonding agent and being directly sealed in. Since bubbles adversely affect physical properties, there is a demand to mitigate this phenomenon.
[0016] The present inventors have elucidated the mechanism of the bubble incorporation and devised a means to eliminate it. Specifically, the present invention can provide the following means.
[0017] Method 1.
[0018] A temporary fixing composition characterized by containing the following (A) to (C) and having a shear rate of 1s at 23°C as measured by a rotational rheometer -1 The viscosity at atmospheric pressure is in the range of 500 to 10000 mPa·s.
[0019] (A) a monofunctional (meth)acrylate having a surface tension in the range of 20 to 30 mN / m at 23°C as measured by a ds / de method based on a pendant drop method
[0020] (B) Multifunctional (meth)acrylate, measured by rotational rheometer at 23°C and a shear rate of 1 s-1 The viscosity at atmospheric pressure is 1000 mPa·s or more, or it is solid at 23°C, or its molecular weight is 500 or more and the viscosity at 23°C and a shear rate of 1s is measured by a rotational rheometer. -1 The viscosity at atmospheric pressure is 100 mPa·s or more and less than 1000 mPa·s
[0021] (C) Photoradical polymerization initiator
[0022] Method 2.
[0023] The temporary fixing composition according to embodiment 1, wherein
[0024] In the mass ratio of the component (A) to the component (B), the amount of the component (A) is in the range of 5 to 65%.
[0025] Method 3.
[0026] The temporary fixing composition according to embodiment 1 or 2, wherein the component (A) is an aliphatic monofunctional (meth)acrylate.
[0027] Method 4.
[0028] The temporary fixing composition according to embodiment 3, wherein the aliphatic group of the component (A) has 6 to 30 carbon atoms.
[0029] Method 5.
[0030] The temporary fixing composition according to any one of aspects 1 to 4, wherein the component (B) contains an oligomer or a polymer.
[0031] Method 6.
[0032] The temporary fixing composition according to any one of aspects 1 to 5, further comprising the following (D).
[0033] (D) UV absorber
[0034] Method 7.
[0035] A cured product comprising the temporary fixing composition according to any one of aspects 1 to 6.
[0036] Method 8.
[0037] The cured product according to aspect 7, wherein the 2% mass loss temperature is 300° C. or higher in a nitrogen atmosphere.
[0038] Method 9.
[0039] A manufacturing method is a method for manufacturing a substrate for electronic equipment, comprising the following steps:
[0040] a step of mixing a monofunctional (meth)acrylate, a polyfunctional (meth)acrylate, and a photoradical polymerization initiator to prepare a composition having a viscosity at 23° C. in the range of 500 to 10,000 mPa·s;
[0041] The step of applying the prepared composition on a silicon wafer by spin coating to achieve a flatness of the surface of the applied composition with a height difference of less than 40 μm; and
[0042] A step of bonding a support to the silicon wafer so as to sandwich the applied composition.
[0043] Method 10.
[0044] A temporary fixing adhesive comprising the temporary fixing composition according to any one of aspects 1 to 6.
[0045] Method 11.
[0046] An adhered article comprising the temporary fixing adhesive according to aspect 10 and base materials adhered by the temporary fixing adhesive.
[0047] Method 12.
[0048] A method for manufacturing a thin wafer using the temporary fixing adhesive according to embodiment 10.
[0049] According to the present invention, a novel composition can be obtained that can reduce the incorporation of bubbles during a spin coating process in the manufacture of electronic devices. DETAILED DESCRIPTION
[0050] In this specification, unless otherwise specified, the numerical range includes its upper limit and lower limit. In this specification, a monofunctional (meth)acrylate refers to a compound having one (meth)acryloyl group in one molecule. A multifunctional (meth)acrylate refers to a compound having two or more (meth)acryloyl groups in one molecule. An n-functional (meth)acrylate refers to a compound having n (meth)acryloyl groups in one molecule. The polymerizable functional group in the multifunctional (meth)acrylate may have only an acryloyl group, only a methacryloyl group, or both an acryloyl group and a methacryloyl group.
[0051] In embodiments of the present invention, a temporary fixing composition (also referred to as a "temporary fixing agent") can be provided, comprising (A) a monofunctional (meth)acrylate having predetermined physical properties, (B) a polyfunctional (meth)acrylate having predetermined physical properties, and (C) a photoradical polymerization initiator, and having a predetermined viscosity overall. The present inventors discovered that during the spin coating process for applying the temporary fixing agent in the manufacture of electronic device substrates, the temporary fixing agent on the substrate undergoes microscopic deformation due to centrifugal force as the substrate rotates. The extent of this microscopic deformation affects the presence or absence of air bubbles, leading to the development of the present invention.
[0052] During the spin coating process, centrifugal force is known to cause a protrusion (called an "edge bead") near the edge of an object. However, in the field of acrylate-based temporary adhesives containing a combination of monofunctional (meth)acrylates and polyfunctional (meth)acrylates, the factors that determine the formation of this edge bead were unknown. Specifically, the authors discovered that if multiple conditions—the combination of the surface tension of the monofunctional (meth)acrylate, the viscosity of the polyfunctional (meth)acrylate, and the viscosity of the mixture—are not met, the edge bead becomes larger. Furthermore, if the edge bead height is 40 μm or less, air bubbles are less likely to enter when bonding the support to the wafer. This discovery led to the solution of the present invention.
[0053] In this specification, the viscosity of the entire composition is measured at 23°C (atmospheric pressure) and a shear rate of 1s by a rotational rheometer. -1 The value when is in the range of 500 to 10000 mPa·s. The viscosity is preferably 500 to 8000 mPa·s, more preferably 500 to 5000 mPa·s. If the viscosity of the entire composition is less than 500 mPa·s, the coating properties are low and cannot be used for practical purposes. In addition, if the viscosity of the entire composition exceeds 10000 mPa·s, the viscosity is too high and is not suitable for spin coating. In addition, in this specification, the viscosity of the following (B) component is also measured in the same manner as above.
[0054] The monofunctional (meth)acrylate as component (A) contained in this composition is characterized by a surface tension of 20 to 30 mN / m at 23°C, as measured by the ds / de method using a pendant drop method. Although hypothetical, it is speculated that if the surface tension of component (A), which forms a relatively flexible skeleton in the composition, is within a narrow, specific range, it interacts with component (B) to resist deformation due to centrifugal force.
[0055] It should be noted that the ds / de method is a method of measuring the maximum diameter (equatorial diameter) de of a hanging drop formed by the pendant drop method and the hanging drop diameter ds at a position only de above the bottom of the hanging drop, and calculating the surface tension γ using the following formula.
[0056] γ=ρg(de) 2 (1 / H)
[0057] Wherein, ρ is density, g is gravitational acceleration, and 1 / H is a correction term obtained from ds / de. The ds / de method is well known, for example, in the following literature.
[0058] https: / / www.scas.co.jp / technical-informations / technical-news / pdf / tn142.pdf
[0059] The type of component (A) can be selected based on the ds / de method. When component (A) contains two or more monofunctional (meth)acrylates, the surface tension of the mixture of the two or more monofunctional (meth)acrylates can be measured and determined. In addition, the surface tension of the entire composition can also be measured in the same way as when component (A) is alone, and is preferably in the range of 28 to 33 mN / m at 23°C. Although it is an assumption, it is believed that the surface tension of the composition is directly proportional to the height of the edge beads described below.
[0060] Component (A) is preferably an aliphatic monofunctional (meth)acrylate. The aliphatic group may have 6 to 30 carbon atoms, more preferably 8 to 20. Although hypothetical, it is speculated that a moderately hydrophobic component (A) will facilitate the aforementioned surface tension effect. Furthermore, it is believed that highly polar monofunctional (meth)acrylates such as acryloylmorpholine generally have excessively high surface tension, making them unsuitable.
[0061] In the mass ratio of the component (A) to the component (B), the amount of the component (A) is preferably in the range of 5 to 65%, more preferably 5 to 60%, and even more preferably 10 to 50%.
[0062] The polyfunctional (meth)acrylate as the component (B) contained in the present composition is characterized in that the shear rate at 23°C measured by a rotational rheometer is 1s -1 The viscosity at atmospheric pressure is 1000 mPa·s or more, or it is solid at 23°C, or its molecular weight is 500 or more and the shear rate at 23°C measured by a rotational rheometer is 1s -1The viscosity at atmospheric pressure is 100 mPa·s or more and less than 1000 mPa·s (preferably 120 mPa·s or more and less than 1000 mPa·s). It should be noted that regarding the above “… at 23°C… the viscosity at atmospheric pressure is 1000 mPa·s or more, or it is solid at 23°C”, the latter is essentially equivalent to a description of the upper limit of the viscosity (that is, being solid can also be interpreted as having very high viscosity). Therefore, it should be noted that although the above description “… at 23°C… the viscosity at atmospheric pressure is 1000 mPa·s or more” does not specify an upper limit, there is no technical ambiguity.
[0063] While not wishing to be bound by a particular theory, it is speculated that by combining component (B), which has a certain viscosity or molecular weight or is solid at room temperature, with component (A), the alkyl groups of component (A) are oriented outwards, exposed on the surface, thereby reducing edge beading. The type of component (B) can be selected based on a viscosity measurement method. When component (B) contains two or more polyfunctional (meth)acrylates, the viscosity of the mixture can be determined.
[0064] The component (B) may be a monomer, or may contain an oligomer or a polymer.
[0065] The photoradical polymerization initiator as the component (C) contained in the present composition refers to a substance that can initiate the radical polymerization of the components (A) and (B) by being irradiated with light, for example, a compound whose molecule breaks and splits into two or more radicals by irradiation with ultraviolet light or visible light (for example, a wavelength of 350 nm to 700 nm, preferably 365 nm to 500 nm, more preferably 385 nm to 450 nm). Examples of photoradical polymerization initiators include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-ylphenyl)-butan-1-one, 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyl oxime, and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime). Component (C) may contain one or more of these, or a combination of two or more.
[0066] (C) component may preferably contain an acylphosphine oxide compound. Preferred acylphosphine oxide compounds include: one or more selected from bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide. As a photo-radical polymerization initiator, it is preferred that it has high sensitivity and light-fading properties and excellent deep curing properties. In addition, it is preferred that the absorption wavelength region for generating free radicals is expanded to a relatively long wavelength region. The absorption wavelength region of the above-mentioned preferred compound is a wavelength range of up to about 440 nm, which is significantly different from the absorption wavelength region of the UV absorber used in the following UV laser stripping process. That is, the degree of UV curing inhibition obtained by the UV absorber is small, and free radical polymerization can be initiated with light of a longer wavelength. Therefore, even in the coexistence of a UV absorber, the effect of initiating free radical polymerization at a relatively fast speed and efficiently, thereby curing, can be obtained.
[0067] In a preferred embodiment, the photoradical polymerization initiator can be selected based on absorbance. Specifically, the photoradical polymerization initiator can be selected from one or more compounds that meet any one or more of the following conditions: when dissolved at a concentration of 0.1% by mass in a solvent that does not have a maximum absorption in the wavelength region of 300 to 500 nm (such as acetonitrile or toluene), the absorbance at a wavelength of 365 nm is 0.5 or more, the absorbance at a wavelength of 385 nm is 0.5 or more, and the absorbance at a wavelength of 405 nm is 0.5 or more. Examples of compounds satisfying such conditions include 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime) having an absorbance of 0.5 or greater at a wavelength of 365 nm when dissolved in acetonitrile as a solvent at a concentration of 0.1% by mass; 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyl oxime having an absorbance of 0.5 or greater at wavelengths of 365 nm and 385 nm; and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide having absorbances of 0.5 or greater at wavelengths of 365 nm, 385 nm, and 405 nm.
[0068] In addition, from the viewpoint of achieving both curability by the photoradical polymerization initiator and UV laser peeling, a double (η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium can also be used as a photoradical polymerization initiator.
[0069] As the photoradical polymerization initiator (C), preferably one or more selected from acylphosphine oxide compounds, titanocene compounds, or α-aminoalkylphenone compounds are preferred in terms of reaction speed, heat resistance after curing, low outgassing, and absorption characteristics in a region different from both the wavelength of the UV laser used for UV laser lift-off described below and the absorption wavelength region of the UV absorber used for UV laser lift-off. Furthermore, in addition to the above, oxime ester compounds can be selected as photoradical polymerization initiators for resin compositions used for temporary fixation purposes in the temporary fixation composition having the structure below, which is intended to prevent damage from the time the substrate to be processed and the support substrate are joined together until the heating step.
[0070] Examples of the acylphosphine oxide-based compounds include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide and 2,4,6-trimethylbenzoyldiphenylphosphine oxide. Among them, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide is particularly preferred.
[0071] Examples of the titanocene-based compounds include: bis(η 5 -2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium.
[0072] Examples of the α-aminoalkylphenone compounds include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one and 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one.
[0073] Examples of oxime ester compounds include 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-O-benzoyloxime and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime). Among these, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime) is preferred.
[0074] In terms of reaction speed, heat resistance after curing, and low outgassing properties, the amount of the photoradical polymerization initiator (C) used is preferably 0.01 to 5 parts by mass, and more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the total of components (A) and (B). If the amount of component (C) is 0.01 parts by mass or greater, sufficient curing properties are achieved, while if it is 5 parts by mass or less, low outgassing properties and heat resistance are less likely to be impaired.
[0075] The present composition may also contain a UV absorber as component (D). A UV absorber is a compound whose molecules, for example, break down, decompose, and vaporize upon irradiation with ultraviolet light or visible light lasers. This decomposition and vaporization occurs at the interface between the supporting substrate (or support) and the temporary bonding agent, thereby losing the adhesive strength between the temporary bonding agent and the supporting substrate (or support) maintained until immediately prior to the peeling step.
[0076] The UV absorber (D) is preferably one or more selected from benzotriazole compounds, benzophenone compounds, and hydroxyphenyltriazine compounds in terms of the degree of overlap between the UV absorption wavelength region and the UV laser wavelength, UV absorption characteristics at the same wavelength, low outgassing properties, and heat resistance.
[0077] As the benzotriazole compound, in terms of compatibility with the resin component, UV absorption properties, low outgassing properties, and heat resistance, particularly preferred are one or more selected from 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2,2'-methylenebis[6-(2H-benzotriazole-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol], 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimide-methyl)-5-methylphenyl]benzotriazole, and 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole.
[0078] As the hydroxyphenyltriazine-based compound, in terms of compatibility with the components (A) and (B), UV absorption properties, low outgassing properties, and heat resistance, at least one selected from 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bis-butoxyphenyl)-1,3,5-triazine, and 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine is particularly preferred.
[0079] As the benzophenone compound, in terms of compatibility with the components (A) and (B), UV absorption properties, low outgassing properties, and heat resistance, at least one selected from 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, 2,2'-dihydroxy-4,4'-diacryloyloxybenzophenone, and hydroxybenzophenone compounds is particularly preferred.
[0080] In an embodiment preferably used in a UV laser lift-off process, the most preferred UV absorber is one or more selected from 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine, 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bis-butoxyphenyl)-1,3,5-triazine, or 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol]. These absorbers have excellent compatibility with component (A), relatively high melting points, and relatively low vapor pressures at temperatures of approximately 300°C or less. Therefore, the amount used can be selected over a wide range, and they contribute to reducing outgassing from the cured temporary fixing composition under these temperature conditions.
[0081] As the UV absorber (D), the absorbers selected based on the UV transmittance listed below are most preferably used. By making the component (D) have such a UV transmittance, the curing and peeling of the composition can be appropriately controlled.
[0082] When the UV absorber is dissolved at a concentration of 0.002% by mass in a solvent that does not have a maximum absorption at a wavelength of 290 to 410 nm, the transmittance at a wavelength of 355 nm with an optical path length of 1 cm is preferably 50% or less, and at a wavelength of 385 to 420 nm, the transmittance is preferably greater than 50%. More preferably, the transmittance at 355 nm is 40% or less, and at a wavelength of 385 to 420 nm, the transmittance can be 60% or greater.
[0083] Preferred UV absorbers (D) from the viewpoint of transmittance under the above conditions include, for example, the following UV absorbers: 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole (RUVA-93 manufactured by Otsuka Chemical Co., Ltd., molecular weight 323.0), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (Tinuvin 900 manufactured by BASF, Adekastab LA-24 manufactured by ADEKA, EVERSORB 76 / EVERSORB 234 manufactured by Everlight Chemical Co., Ltd., molecular weight 447), 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (Tinuvin 928 manufactured by BASF, EVERSORB manufactured by Everlight Chemical Co., Ltd. 89 / 89FD, molecular weight 442), 2-[4-[(2-hydroxy-3-(2'-ethyl)hexyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine (Tinuvin 405 manufactured by BASF, molecular weight 584), and 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bis-butoxyphenyl)-1,3,5-triazine (Tinuvin 460 manufactured by BASF, molecular weight 630).
[0084] The UV transmittance of a cured product herein is a value obtained by reflectivity spectrometry. Specifically, the transmittance can be obtained using a reflectivity spectrometer (V-650 manufactured by JASCO Corporation) using a film of the cured product having a thickness of approximately 50 μm sandwiched between sheets of PET resin under the following conditions.
[0085] Slot length: 10mm
[0086] Metering mode: T (Transmittance)
[0087] Measuring range: 450-200nm
[0088] Data scanning interval: 1nm
[0089] UV / visible band width: 2.0nm
[0090] Sensing: medium
[0091] Scanning speed: 40nm / min
[0092] Light source switching: 340nm
[0093] Light source: D2 / WI
[0094] Filter switching: Step
[0095] Calibration: Baseline
[0096] The amount of the UV absorber as component (D) is preferably 0.01 to 5 parts by mass, more preferably 0.5 to 2.5 parts by mass, relative to 100 parts by mass of the total of components (A) and (B). If it is 0.01 parts by mass or more, a sufficient UV laser stripping rate can be obtained, while if it is 5 parts by mass or less, the effects of low outgassing and less impairment of heat resistance can be achieved.
[0097] The weight average molecular weight in this specification is a value converted to standard polystyrene measured by gel permeation chromatography (GPC). Specifically, the weight average molecular weight can be determined under the following conditions using tetrahydrofuran as a solvent and a GPC system (SC-8010 manufactured by Tosoh Corporation) using a commercially available standard polystyrene to prepare a calibration curve.
[0098] Flow rate: 1.0ml / min
[0099] Set temperature: 40℃
[0100] Column configuration: 1 "TSK guardcolumn MP (×L)" manufactured by Tosoh Corporation, 6.0 mm ID × 4.0 cm, and 2 "TSK-GELMULTIPORE HXL-M" manufactured by Tosoh Corporation, 7.8 mm ID × 30.0 cm (theoretical plate number 16,000), for a total of 3 columns (total theoretical plate number 32,000)
[0101] Sample injection volume: 100 μl (test solution concentration 1 mg / ml)
[0102] Infusion pressure: 39kg / cm 2
[0103] Detector: RI detector (differential refractive index detector)
[0104] In one embodiment of the present invention, a cured product of the above-mentioned composition is also provided. Such curing can be performed using the following light source. When the cured product is formed into a cured film having a thickness of 50 μm, it preferably satisfies one or more of the following conditions, and more preferably satisfies all of them. The following conditions can be satisfied, for example, by using a UV absorber.
[0105] The light transmittance of the cured film is 70% or more in a wavelength range of 395 nm or more among the wavelengths of the light source used for curing.
[0106] The light transmittance of the cured film is 20% or more in a wavelength range of 385 nm or more and less than 395 nm among the wavelengths of a light source used for curing.
[0107] The light transmittance of the cured film is 1% or less at the wavelength (355 nm) of UV laser light used for UV laser lift-off.
[0108] Meeting these requirements allows for both practically high curing speeds and UV laser stripping speeds. Furthermore, in addition to achieving both high curing and UV laser stripping speeds, the rate of mass loss under post-curing heating conditions can be reduced (or the amount of outgassing under high-temperature vacuum conditions can be reduced). A temporary bonding agent with these characteristics is particularly suitable for use in post-thinning backside processes, including high-temperature vacuum processes such as electrode formation using ion implantation, annealing, or sputtering.
[0109] The present composition can be used as a temporary fixing resin composition, a temporary fixing adhesive, an adhesive sheet, or a temporary fixing adhesive for electronic device manufacturing. In this specification, the temporary fixing composition, temporary fixing resin composition, and temporary fixing adhesive are sometimes collectively referred to as a temporary fixing agent.
[0110] When the present composition is used to bond a substrate to be processed to an optically transparent supporting substrate (or support), it is preferred that the energy be 1 to 20,000 mJ / cm in the visible or ultraviolet region (the wavelength or central wavelength is preferably 350 to 405 nm, more preferably 365 to 405 nm, and most preferably 385 to 405 nm). 2 If the energy is 1mJ / cm 2 If the above, sufficient adhesion can be obtained, if it is 20000mJ / cm 2 The productivity is excellent, the decomposition products from the photo-radical polymerization initiator are not easily generated, and the generation of outgassing is suppressed. In terms of productivity, adhesion, low outgassing, and easy peeling, 1000 to 10000 mJ / cm 2 .
[0111] The substrates bonded by this composition are not particularly limited, but preferably at least one substrate is a light-transmitting, transparent substrate. Examples of transparent substrates include inorganic substrates such as crystal, glass, quartz, calcium fluoride, and magnesium fluoride; and organic substrates such as plastics. Inorganic substrates are preferred due to their versatility and ability to achieve significant results. Among inorganic substrates, at least one selected from glass and quartz is preferred.
[0112] This composition can be photocurable, resulting in a cured product exhibiting excellent heat resistance and peelability. In one embodiment, the cured product of the composition of the present invention exhibits minimal outgassing even when exposed to high temperatures, making it suitable for bonding, sealing, and coating various optical components, optical devices, and electronic components. The composition of the present invention is suitable for applications requiring durability in various aspects, including solvent resistance, heat resistance, and adhesion, and is particularly well-suited for use in semiconductor manufacturing processes.
[0113] The cured product of the present composition can be used in processes in a wide temperature range from room temperature to high temperature. The heating temperature in the process is preferably below 350°C, more preferably below 300°C, and most preferably below 250°C. In a preferred embodiment, the temperature at which the heating mass reduction rate of the cured product becomes 2% may be above 250°C. The adhesive bonded by the present composition has a high shear adhesion, so it can withstand thinning processes, etc., and can be easily peeled off after heating processes such as insulating film formation. In the case of use at high temperatures, the cured product of the present composition can be used, for example, in processes at high temperatures preferably above 200°C, more preferably above 250°C.
[0114] In one embodiment, an adhesive is provided that is bonded to a substrate using the composition as an adhesive. The adhesive can be peeled off by applying an external force. For example, the adhesive can be peeled off by inserting a knife, sheet, or wire into the bonded portion. Alternatively, the adhesive can be peeled off by irradiating the entire surface of the optically transparent substrate side of the adhesive with a UV laser or an IR laser in a scanning manner.
[0115] <Thin Wafer Manufacturing Method>
[0116] In one embodiment, a method for manufacturing a thin wafer is provided. This method is characterized by using the aforementioned temporary fixing composition or temporary fixing adhesive (hereinafter sometimes simply referred to as an adhesive or temporary fixing agent) as an adhesive layer between a wafer having a semiconductor circuit, etc., and a support. This method for manufacturing a thin wafer comprises the following steps (a) to (e).
[0117] [Step (a)]
[0118] Process (a) is a process in which the circuit-forming surface of a chip having a circuit-forming surface on the surface and a circuit-non-forming surface on the back is bonded to a support body via an adhesive, the adhesive is applied to the support body or the chip with the circuit by a spin coating method, and another support body or chip with the circuit is bonded under vacuum.
[0119] A wafer having a circuit-forming surface and a non-circuit-forming surface is a wafer having one surface for forming a circuit and the other surface for not forming a circuit. The wafer to which the present invention is applicable is typically a semiconductor wafer. Examples of such semiconductor wafers include, but are not limited to, silicon wafers. Examples include gallium nitride wafers, lithium tantalate wafers, lithium niobate wafers, silicon carbide wafers, germanium wafers, gallium-arsenic wafers, gallium-phosphorus wafers, and gallium-arsenic-aluminum wafers. The thickness of the wafer is not limited, but is preferably 600 to 800 μm, more preferably 625 to 775 μm. For example, a light-transmitting transparent substrate is used as the support.
[0120] [Step (b)]
[0121] Step (b) is a step of photocuring the adhesive. After forming the above-mentioned wafer processed body (laminated substrate), it is preferably subjected to light curing in the visible or ultraviolet region (wavelength or center wavelength is preferably 350 to 405 nm, more preferably 365 to 405 nm, and most preferably 385 to 405 nm) at an energy of 1 to 20,000 mJ / cm 2 If the energy is 1mJ / cm 2 If the above, sufficient adhesion can be obtained, if it is 20000mJ / cm 2 The productivity is excellent, the decomposition products from the photo-radical polymerization initiator are less likely to be generated, and the outgassing is also suppressed. In terms of productivity, adhesion, low outgassing, and easy peeling, 1000 to 10000 mJ / cm is more preferable. 2 .
[0122] When curing the composition, a black light, UV-LED, or visible light-LED can be used as a light source. For example, the following light sources can be used. Regardless of the center wavelength, a black light containing a component with a wavelength of 385 nm or longer is preferably used. When a wavelength range is described in this specification, whether the wavelength is within the range is determined by whether the center wavelength is within the range.
[0123] Black light (center wavelength 365nm, illumination 10mW / cm 2 , TUV-8271 manufactured by TOYO ADTEC Co., Ltd.)
[0124] UV-LED (wavelength 385±5nm, illumination 350mW / cm 2 (Conditions: Working distance 20 mm from the front end of the mirror unit, HOYA H-4MLH200-V2-1S19 + dedicated mirror unit)
[0125] UV-LED (wavelength 395±5nm, illumination 375mW / cm 2(Conditions: Working distance 20 mm from the front end of the mirror unit, HOYA H-4MLH200-V3-1S19 + specially designed mirror unit)
[0126] UV-LED (wavelength 405±5nm, illumination 400mW / cm 2 (Conditions: Working distance 20 mm from the front end of the mirror unit, HOYA H-4MLH200-V4-1S19 + dedicated mirror unit)
[0127] UV-LED (Central wavelength 405nm, illumination 10mW / cm 2 , HLDL-120V0-NWPSC made by CCS)
[0128] Visible light-LED (wavelength 451±5nm, illumination 550mW / cm 2 (Conditions: Working distance 10 mm from the front end of the irradiation unit, HLDL-155VL450-PSC manufactured by CCS)
[0129] Visible light-LED (wavelength 492±5nm, illumination 400mW / cm 2 (Conditions: Working distance 10 mm from the front end of the irradiation unit, HLDL-155BG-PSC manufactured by CCS)
[0130] In a preferred embodiment, because the irradiation wavelength is generally broad, UV-LEDs or visible light-LEDs can be used as light sources, as they require less cumulative light (shorter irradiation times) than black lights, which tend to have longer irradiation times due to their high cumulative light intensity. Specifically, by using an LED light source with a narrow irradiation wavelength band, temporary fixing can be performed in a shorter time, resulting in a reduction in the time required for the manufacturing process.
[0131] [Step (c)]
[0132] Step (c) is a step of grinding and / or polishing the non-circuit forming surface of the wafer bonded to the support, that is, a step of grinding the back side of the wafer of the wafer processed body obtained by bonding in step (a) to thin the thickness of the wafer. The thickness of the thinned wafer is preferably 10 to 300 μm, more preferably 30 to 100 μm. There is no particular restriction on the method of grinding / polishing the back side of the wafer, and a known grinding / polishing method can be used. Regarding grinding, it is preferred to pour water on the wafer and the grindstone (a grindstone with a diamond knife, etc.) and grind while cooling.
[0133] [Step (d)]
[0134] Process (d) is a process for grinding / polishing the non-circuit forming surface of the wafer processing body, that is, a process for processing the non-circuit forming surface of the wafer processing body thinned by back grinding / polishing. This process includes various processes used at the wafer level. For example, electrode formation, metal wiring formation, protective film formation, etc. can be mentioned. More specifically, there can be mentioned metal sputtering for forming electrodes, etc.; wet etching for etching the metal sputtering layer; pattern formation by coating, exposing, and developing a resist for making a shield for metal wiring formation; stripping of the resist; dry etching; formation of metal plating; silicon etching for forming TSV; and formation of an oxide film on the silicon surface, etc., which are processes known to date.
[0135] [Step (e)]
[0136] Step (e) is a peeling step. This step is a step of peeling the wafer processed in step (d) from the wafer processing body. For example, it is a step of peeling the wafer from the wafer processing body before dicing after various processes have been performed on the thinned wafer. In this case, a wafer dicing tape can be affixed to the thinned and processed surface in advance. This peeling step is usually carried out under relatively low temperature conditions ranging from room temperature to about 60°C. As this peeling step, any of the well-known UV laser peeling steps, IR laser peeling steps, or mechanical peeling steps can also be used.
[0137] The UV laser stripping process involves irradiating the entire surface of the wafer body with a UV laser, for example, by scanning back and forth linearly along a tangential direction from the end of the wafer body on the optically transparent support side. The laser energy decomposes the adhesive layer, leading to stripping. This stripping process is described, for example, in Japanese Patent Publication No. 2019-501790 or Japanese Patent Publication No. 2016-500918.
[0138] The IR laser stripping process refers to the following process: for example, the entire surface of the wafer processing body is irradiated with IR laser in a manner of scanning back and forth in a straight line along the tangential direction from the end of the optically transparent support body side of the wafer processing body, and the adhesive layer is heated and decomposed by the energy of the laser, thereby stripping. Such a stripping process is described in, for example, Japanese Patent Gazette No. 4565804. In order to implement this IR laser stripping process, a light-to-heat conversion layer (for example, 3M's LTHC, Light-To-Heat-Conversion release coating) that absorbs IR laser and converts it into heat can also be provided between the temporary fixing agent layer and the glass support body. When using 3M's LTHC, for example, the LTHC is spin-coated on the glass support body and cured. Then, after the temporary fixing agent layer is spin-coated on the wafer, it can be bonded to the above-mentioned glass support body on which the LTHC layer is formed and UV cured. Regarding the method of implementing the IR laser stripping process using 3M's LTHC, for example, it is described in the same Japanese Patent Gazette No. 4565804 as mentioned above.
[0139] The mechanical peeling process includes, for example, inserting a scraper into the interface end of the wafer processing body to create a crack between the wafer and the support. The wafer processing body is positioned horizontally with the wafer facing downward. After the scraper is inserted, an upward stress is applied to the upper support and / or the scraper to promote the crack and thereby peel the wafer from the support. Such a peeling process is described, for example, in Japanese Patent No. 6377956 or Japanese Patent Application Laid-Open No. 2016-106404.
[0140] When peeling the present composition, any of these peeling methods can be used. In this case, it is preferred to fix one of the wafers or supports of the wafer processing body horizontally, insert a scraper or use a solvent (for example, aliphatic or aromatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.) to swell the periphery of the adhesive layer to form the starting point of peeling, and then lift the other side at a certain angle from the horizontal direction. These peeling methods are usually carried out at room temperature, and are preferably heated to an upper limit of about 90°C. When using a laser, it is preferred to use a YAG laser or a YVO4 laser.
[0141] In the case of a mechanical peeling step, the step of peeling the wafer processed in the step (e) from the support preferably further includes the following step:
[0142] (f) bonding a wafer dicing tape to a wafer surface of the processed wafer;
[0143] (g) vacuum-adsorbing the wafer dicing tape surface onto the adsorption surface;
[0144] (h) The support body is peeled off from the processed wafer while the temperature of the adsorption surface is in the temperature range of 10 to 100°C.
[0145] In this manner, the support body can be easily peeled off from the processed wafer, and the subsequent wafer dicing step can be easily performed.
[0146] In addition, when the lift-off is performed using a UV laser or an IR laser, the manufacturing method preferably further includes, for example, the following steps:
[0147] (i) placing / fixing the processed wafer with the optically transparent support side facing upward in a horizontal position, preferably using wafer dicing tape;
[0148] (j) The entire surface of the processed wafer is irradiated with laser light in a scanning manner from the support side of the wafer.
[0149] In this manner, the support body can be easily peeled off from the processed wafer, and the subsequent wafer dicing step can be easily performed.
[0150] In addition, after the step of peeling the wafer processed in step (e) from the support using UV laser or IR laser, the following steps need to be performed:
[0151] (k) Removing the temporary fixing agent remaining on the wafer surface.
[0152] Methods for removing the temporary bonding agent include: applying an adhesive tape, such as wafer dicing tape, to the entire surface of the other side where the temporary bonding agent remains, while vacuum-adhering the thinned surface to the adsorption surface, and then peeling off the tape along with the temporary bonding agent; or immersing the wafer in a solvent (e.g., aliphatic or aromatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, and mesitylene) to swell the adhesive layer and then peeling it off. Of these methods, the tape peeling method is preferred due to the reduced number of steps and time required.
[0153] After removing the temporary fixative, the wafer can also be directly processed without cleaning the surface. In the case of cleaning, it is preferred to further perform the following steps:
[0154] (l) The support and the chip from which the temporary fixing agent has been removed are cleaned with a solvent (e.g., an aliphatic or aromatic hydrocarbon solvent such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.) with the circuit-forming surface facing upward.
[0155] After the temporary fixing agent is removed in step (k), some adhesive (temporary fixing agent) may remain on the circuit-forming surface of the wafer. Furthermore, while the peeled support is preferably cleaned and reused, adhesive residue may remain on the surface of the support. Methods for removing this adhesive residue include immersing the wafer in a solvent (e.g., aliphatic or aromatic hydrocarbon solvents such as pentane, hexane, heptane, octane, nonane, decane, benzene, toluene, xylene, mesitylene, etc.) to cause the wafer to swell and then peel.
[0156] In one embodiment, when the composition is cured to obtain a cured product, various methods as described below can be employed.
[0157] As a first method, a layer composed of a temporary fixing composition containing the above-mentioned components is cured to obtain a single-layer cured product.
[0158] Then, as a second method, the following method can be cited: prepare a first layer composed of a temporary fixing composition containing at least (A) to (C) components and not containing a UV absorber as component (D), and a second layer composed of a temporary fixing composition containing at least (A) to (D) components, and cure them to obtain an integrated single-layer or multi-layer (complex) cured product. In the cured product, it is preferred that the concentration distribution of the components in the thickness direction is different, or the concentration distribution of the components in the upper surface and the lower surface in the thickness direction of the cured product is different. The difference in the concentration distribution of the components can be confirmed by quantifying the UV transmittance of both sides of the cured product using the above-mentioned reflectivity measurement spectrometry. By this method, layers with different light transmittance are combined, thereby achieving the most preferred curing effect. In addition, during the above-mentioned curing, a black light lamp or UV-LED (the same applies to the following method) can be used as a light source. As an example of a black light lamp, TUV-8271 (central wavelength 365nm, illuminance 10mW / cm2) manufactured by TOYO ADTEC Co., Ltd. can be cited. 2 ). In addition, as UV-LED, there can be cited: H-4MLH200-V2-1S19+special design mirror unit (wavelength 385±5nm, illumination 350mW / cm 2 , conditions: scanning distance from the front end of the mirror unit 20mm), HOYA Corporation H-4MLH200-V3-1S19 + dedicated design mirror unit (wavelength 395±5nm, illumination 375mW / cm 2 , conditions: working distance from the front end of the mirror unit 20mm), HOYA Corporation H-4MLH200-V4-1S19 + dedicated design mirror unit (wavelength 405±5nm, illumination 400mW / cm 2 , condition: working distance from the front end of the mirror unit is 20mm).
[0159] Alternatively, as a third method, a multilayer cured product can be obtained by placing a layer of a commercially available LTHC agent (light-to-heat conversion agent) on a layer of a temporary fixing composition containing at least components (A) to (C) and curing the layer. This method can easily produce a cured product.
[0160] The cured product obtained by the above-mentioned method can be combined with an adherend to provide a structure.
[0161] Various examples of methods for producing the aforementioned structure can be cited. For example, a first production method may include the following steps: applying a first temporary fixing composition containing at least components (A) to (C) and no component (D) on a wafer and partially curing the composition; applying a second temporary fixing composition containing at least components (A) to (D) on the partially cured temporary fixing composition; and further placing a transparent substrate on the applied second temporary fixing composition and photocuring the composition.
[0162] In addition, the second method for manufacturing the structure may include the following steps: applying a first temporary fixing composition containing at least components (A) to (C) and not containing component (D) on a wafer and partially curing the composition as needed; applying a second temporary fixing composition containing at least components (A) to (D) on a transparent substrate and partially curing the composition as needed; and bringing the wafer and the transparent substrate, respectively coated with the temporary fixing composition, into close contact with each other and then bonding them by photocuring.
[0163] Unlike the aforementioned temporary fixing composition, the same composition used in the temporary fixing composition of the present invention can also be used as a raw material for the light-to-heat conversion (LTHC) layer described in Japanese Patent No. 4565804, which absorbs IR laser light and converts it into heat. Adding this composition as a component of the light-to-heat conversion (LTHC) layer can improve its heat resistance.
[0164] In one embodiment, a method for manufacturing a semiconductor wafer can be provided, comprising the steps of applying a temporary fixing composition to a semiconductor wafer substrate and / or a support member to bond the semiconductor wafer substrate to the support member; curing the temporary fixing adhesive by irradiating the adhesive with light having a wavelength of 350 to 700 nm (preferably 365 to 500 nm, more preferably 385 to 450 nm) to obtain an adhesive; and irradiating the adhesive with a laser having a wavelength less than 385 nm (preferably a laser having a wavelength of 200 nm or greater and less than 385 nm) to release the semiconductor wafer substrate. Both the curing and release steps of this manufacturing method are performed at room temperature, do not require heating or cooling components, and generally do not require the use of solvents, resulting in simplicity and a short cycle time.
[0165] Furthermore, the cured temporary fixing adhesive may also constitute a single layer in the adhesive, thereby simplifying the process and shortening the production time.
[0166] In a preferred embodiment, by making the composition simultaneously contain the above-mentioned photoradical polymerization initiator of component (C) and the UV absorber of component (D), even a single-layer temporary fixing adhesive can have both a fast curing speed and a fast peeling speed. Furthermore, the uncured UV curable monomer component remaining in the cured product when the temporary fixing adhesive is UV cured can be significantly reduced, the heat resistance of the cured product can be improved, and the volatilization amount in a nitrogen environment can be reduced. That is, for example, the 2% heating mass reduction temperature of the cured product during Tg / DTA measurement can be increased. Temporary fixing adhesives with high heat resistance of the cured product or reduced volatilization amount in a nitrogen environment are extremely useful for current semiconductor manufacturing processes. The 2% mass reduction temperature of the cured product in a nitrogen environment is preferably above 300°C, preferably above 320°C, and more preferably above 326°C.
[0167] In one embodiment, a method for manufacturing a substrate for an electronic device may be provided. The manufacturing method may include the following steps: mixing a monofunctional (meth)acrylate, a multifunctional (meth)acrylate, and a photoradical polymerization initiator to prepare a composition having a viscosity in the range of 500 to 10,000 mPa·s at 23°C; applying the prepared composition on a silicon wafer by spin coating to achieve a flatness of the surface of the coated composition having a height difference of only 40 μm or less; and bonding a support to the silicon wafer in a manner that sandwiches the coated composition. In this specification, the flatness of the composition surface is measured after coating and curing using a spin coater under the conditions described in the following examples.
[0168] Example
[0169] Hereinafter, the present invention will be described in further detail based on Examples and Comparative Examples, but the present invention is not limited thereto.
[0170] Unless otherwise specified, experiments were conducted at 23°C and 50% humidity. Curable resin compositions (hereinafter sometimes referred to as liquid resin compositions) having the compositions shown in the following table (units are parts by mass) were prepared and evaluated. The following compounds were selected as the components.
[0171] [Table 1]
[0172]
[0173] [Table 2]
[0174]
[0175] (composition)
[0176] The following components were used as component (A). The surface tension value was measured at 23° C. by the ds / de method using “OCA20” manufactured by Eiko Seiki Co., Ltd. The surface tension of the entire composition was measured in the same manner.
[0177] LA: Lauryl acrylate ("LA" manufactured by Osaka Organic Chemical Industry Co., Ltd., surface tension 29.3 mN / m)
[0178] NOAA: n-octyl acrylate ("NOAA" manufactured by Osaka Organic Chemical Industry Co., Ltd., surface tension 27.5 mN / m)
[0179] INAA: Isononyl acrylate ("INAA" manufactured by Osaka Organic Chemical Industry Co., Ltd., surface tension 27.5 mN / m)
[0180] ISTA: Isostearyl acrylate ("ISTA" manufactured by Osaka Organic Chemical Industry Co., Ltd., surface tension 26.3 mN / m)
[0181] ACMO: Acryloylmorpholine (“ACMO” manufactured by KJ Chemicals, surface tension 44.6 mN / m)
[0182] The following components were used as component (B): The viscosity value or the solid state means the viscosity value at 23°C or the solid state at 23°C.
[0183] HX-620: Caprolactone-modified hydroxypivalate neopentyl glycol diacrylate ("Kayarad HX-620" manufactured by Nippon Kayaku Co., Ltd., m+n≒4, (average) molecular weight 768, viscosity 290 mPa·s)
[0184] HX-220: Caprolactone-modified hydroxypivalate neopentyl glycol diacrylate ("Kayarad HX-220" manufactured by Nippon Kayaku Co., Ltd., m+n≒2, (average) molecular weight 541, viscosity 120 mPa·s)
[0185] A-BPEF-2: 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene diacrylate ("NK ESTERA-BPEF-2" manufactured by Shin-Nakamura Chemical Industry Co., Ltd., molecular weight 546, high viscosity exceeding the detection limit, estimated to be more than 1000 mPa·s)
[0186] RA-341: Multifunctional methacrylate polymer ("ART CURE RA-341" manufactured by Negami Industry Co., Ltd.; weight-average molecular weight of the dry polymer is approximately 70,000, exceeding the measurable limit and exhibiting high viscosity, with the viscosity estimated to be greater than 1,000 mPa·s)
[0187] A-BPE-2: Ethoxylated bisphenol A diacrylate ("NK ESTER A-BPE-2" manufactured by Shin-Nakamura Chemical Industry Co., Ltd., wherein R = -CH2CH2O-, m = n = 1, molecular weight 422, solid at 23°C)
[0188] [Chemical Formula 1]
[0189]
[0190] RC100C: Acrylate polymer having acryloyl groups at both ends ("Kaneka XMAPRC100C" manufactured by Kaneka Corporation, having the following structural formula, a (weight average) molecular weight of 24,000, and a high viscosity exceeding the measurement limit, determined to be greater than 1,000 mPa·s)
[0191] [Chemical Formula 2]
[0192]
[0193] As other components, the following components were used as comparative examples.
[0194] Tetrax 6T: Polyisobutylene ("TETRAX Grade 6T" manufactured by ENEOS, viscosity-average molecular weight 60,000)
[0195] A-DCP: tricyclodecane dimethanol diacrylate ("NK ESTER A-DCP" manufactured by Shin-Nakamura Chemical Industry Co., Ltd., molecular weight 304, viscosity 160 mPa·s)
[0196] DCP: tricyclodecane dimethanol diacrylate ("NK ESTER DCP" manufactured by Shin-Nakamura Chemical Industry Co., Ltd., molecular weight 332, viscosity 130 mPa·s)
[0197] (C) Components used were as follows.
[0198] Bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide ("Irgacure 819" manufactured by BASF)
[0199] The following components were used as the component (D).
[0200] 2,4-bis(2-hydroxy-4-butoxyphenyl)-6-(2,4-bis-butoxyphenyl)-1,3,5-triazine ("Tinuvin 460" manufactured by BASF)
[0201] Hydroxyphenyltriazine-based UV absorber ("Tinuvin 479" manufactured by BASF)
[0202] 2-(2'-Hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole ("RUVA-93" manufactured by Otsuka Chemical Co., Ltd.)
[0203] (Liquid sample preparation)
[0204] The materials were mixed and heated at 80°C to form a uniform mixture. The viscosity of each component and the entire composition was measured using a rotational rheometer MCR302 manufactured by Anton-Paar using a cone and plate CP50-2 at a temperature of 23°C and a shear rate of 1 s -1 It should be noted that when measuring the viscosity of the component (B) and the polyfunctional (meth)acrylate of the comparative example, under the above-mentioned measurement conditions, the rotational rheometer could not fully measure the viscosity due to the viscosity being too high, and the viscosity was clearly determined to be higher than 1000 mPa·s (presumably a high viscosity exceeding 100,000 mPa·s).
[0205] (Determination of 2% mass loss temperature)
[0206] The liquid resin composition homogenized by the above-mentioned heating and mixing was sandwiched between PET films and extruded and stretched to a thickness of 70 μm. 2 During the curing process, a UV-LED (central wavelength 405 nm, illumination 100 mW / cm 2 , wafer UV irradiator MUVBA-0.4×0.6×0.2-0010 manufactured by Aitec System Co., Ltd.
[0207] A 10 mg sample of the cured product was measured using a NETZSCH Japan differential thermal mass analyzer (STA-2500). The temperature was raised from room temperature to 600°C at a rate of 10°C / min under a nitrogen flow at a carrier gas flow rate of 70 ml / min. The cured product was then weighed. The heating mass loss rate (2% mass loss temperature) under a nitrogen atmosphere was calculated from this.
[0208] (Evaluation of Vacuum Heat Resistance)
[0209] The prepared liquid resin composition was used to bond a 4-inch silicon wafer (10 cm in diameter × 525 μm thick) to a 4-inch glass wafer (10 cm in diameter × 0.7 mm thick) as a 4-inch sample. During bonding, the thickness of the resin composition was adjusted by adding 0.1% by mass of glass beads (trade name SPL-70, average particle size 70 μm) manufactured by Unitika to the temporary fixing agent and mixing. After bonding, the LED cumulative light intensity was 5000 mJ / cm 2 (Central wavelength 405nm, illumination 100mW / cm 2 ) were used to cure the sample. During the curing process, a UV-LED (central wavelength 405 nm, illumination 100 mW / cm 2 The vacuum heat resistance of the obtained bonded samples was evaluated using a wafer UV irradiator MUVBA-0.4×0.6×0.2-0010 manufactured by Aitec System Co., Ltd. The following vacuum heat resistance was also evaluated for the obtained bonded samples.
[0210] Each bonded sample was placed in a vacuum hot plate chamber and heated at 300° C. and 20 Pa for 1 hour. Thereafter, the peripheral edge of the silicon wafer was visually observed and evaluated according to the following criteria.
[0211] Excellent: No peeling at the end.
[0212] Good: The length of the peeled portion at the end is less than 5 mm from the edge.
[0213] Acceptable: The length of the peeled portion at the end is more than 5 mm and less than 10 mm from the edge.
[0214] Unqualified: The length of the peeled portion at the end is more than 10 mm from the edge.
[0215] (Evaluation of laser peeling properties)
[0216] For the 4-inch bonded sample produced in the above manner, a UV laser was irradiated onto a 210 mm square area with the test body fixed in the center, scanning the entire surface of the test body from the glass support side. The UV laser irradiation conditions are shown below. The UV laser used was the "MD-U1020C" manufactured by KEYENCE. Irradiation was performed under the conditions of 2.5 W output, 40 kHz frequency, 72 μm beam diameter, 150 μm scanning pitch, and 6 m / sec scanning speed. The peelability after irradiation was evaluated using the following definition.
[0217] The condition in which there was no tackiness and the glass support could be easily peeled off from the temporary fixing agent by hand was evaluated as "excellent".
[0218] The state in which the glass support body could be peeled off from the temporary bonding agent by hand while the adhesiveness remained was evaluated as "good".
[0219] The glass support body that could not be peeled off from the temporary bonding agent by hand was evaluated as "failed".
[0220] (Evaluation of edge bead height)
[0221] 6.5 to 7.5 g of the prepared resin composition was applied to an 8-inch Si wafer using a spin coater (MS-A300 manufactured by Mikasa Corporation). After low-speed spinning (50 rpm x 15 sec), the liquid was evenly distributed by high-speed spinning under the following conditions. The upper surface was moved into a glass chamber, and the chamber was replaced with a nitrogen atmosphere. The LED cumulative light intensity was 8100 mJ / cm 2 (Central wavelength 405nm, illumination 45mW / cm 2 ) conditions. Measure the thickest part of the edge and the part 2 cm or more inside the edge, and use the difference as the height of the edge bead.
[0222] High-speed rotation conditions
[0223] Spin time: 15 seconds
[0224] Rotation speed: Nrpm (Using the viscosity value, the rotation speed that gives a thickness of 74 to 76 μm when the coating time is 15 seconds in the following formula)
[0225] Coating amount: 6.5~7.5g
[0226] Calculation formula
[0227] h=h0 / {1+t×(4ω 2 h0 2 / 3ν)} 1 / 2
[0228] h: film thickness [mm], h0: initial film thickness [mm], ω: rotation speed [rad / sec],
[0229] t: time [sec], ν: kinematic viscosity [mm 2 / sec]
[0230] Rotation speed
[0231] ω=πN / 30
[0232] ω: Rotational speed [rad / sec], rotational speed [rpm]
[0233] Kinematic viscosity
[0234] ν=μ / ρ
[0235] ν: dynamic viscosity [m 2 / sec], μ: viscosity [Pa·s], ρ: density [kg / m 3 ]
[0236] Initial film thickness
[0237] h0={w / (s×ρ)}×10
[0238] h0: initial film thickness [mm], w: coating amount [g], s: wafer area [cm 2 ], ρ: density [g / cm 3 ]
[0239] Based on the above results, the compositions of the examples of the present invention all suppressed edge bead height to below 40 μm and exhibited excellent laser peelability and heat resistance. On the other hand, the edge bead heights of Comparative Examples 1 and 2, which lack component (A), were higher, failing to prevent the incorporation of bubbles. The edge bead heights of Comparative Examples 3 and 5, which did not meet the surface tension requirements of component (A), were also higher. Comparative Example 4, which lacked component (B), exhibited poor laser peelability and was unsuitable for practical use.
Claims
1. A temporary fixing composition, characterized in that: Containing the following (A) to (C), and measured by a rotational rheometer at 23°C and a shear rate of 1 s -1 The viscosity at atmospheric pressure is in the range of 500 to 10000 mPa·s; (A) a monofunctional (meth)acrylate having a surface tension in the range of 20 to 30 mN / m at 23° C. as measured by a ds / de method based on a pendant drop method, (B) Multifunctional (meth)acrylate, measured by rotational rheometer at 23°C and a shear rate of 1 s -1 The viscosity at atmospheric pressure is 1000 mPa·s or more, or it is solid at 23°C, or its molecular weight is 500 or more and the viscosity at 23°C and a shear rate of 1 s measured by a rotational rheometer is -1 The viscosity at atmospheric pressure is 100 mPa·s or more and less than 1000 mPa·s, (C) Photoradical polymerization initiator.
2. The temporary fixing composition according to claim 1, wherein In the mass ratio of the component (A) to the component (B), the amount of the component (A) is in the range of 5 to 65%.
3. The temporary fixing composition according to claim 1 or 2, wherein (A) Component is an aliphatic monofunctional (meth)acrylate.
4. The temporary fixing composition according to claim 3, wherein The aliphatic group of the component (A) has 6 to 30 carbon atoms.
5. The temporary fixing composition according to any one of claims 1 to 4, wherein The component (B) includes an oligomer or a polymer.
6. The temporary fixing composition according to any one of claims 1 to 5, further comprising the following (D): (D) UV absorber. 7 . A cured product, which is a cured product of the temporary fixing composition according to claim 1 .
8. The cured product according to claim 7, wherein the 2% mass loss temperature is 300°C or higher in a nitrogen atmosphere.
9. A manufacturing method is a manufacturing method for a substrate for an electronic device, comprising the following steps: A step of mixing a monofunctional (meth)acrylate, a polyfunctional (meth)acrylate and a photoradical polymerization initiator to prepare a composition having a viscosity at 23° C. in the range of 500 to 10000 mPa·s; The step of applying the prepared composition on a silicon wafer by spin coating to make the surface of the applied composition have a flatness with a height difference of only 40 μm or less; and A step of bonding a support to the silicon wafer so as to sandwich the applied composition. 10 . A temporary fixing adhesive comprising the temporary fixing composition according to claim 1 . 11 . An adhered article comprising the temporary fixing adhesive according to claim 10 and a base material adhered by the temporary fixing adhesive.
12. A method for manufacturing a thin wafer, using the temporary fixing adhesive according to claim 10.