Hard alloy, and coated tool and cutting tool using same

By adding a specific proportion of Zr and Nb to the cemented carbide coated tool and forming a multi-layer coating on its surface, the problem of coating peeling caused by differential thermal expansion is solved and the heat resistance and resistance of the cemented carbide are improved. Wear resistance, extending the service life of the tool.

CN118786233APending Publication Date: 2024-10-15KYOCERA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380021031.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-03
Filing Date
2023-02-01
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing carbide-coated tools are prone to coating peeling due to poor thermal expansion at high temperatures, resulting in insufficient wear resistance and durability.

Method used

A cemented carbide containing a hard phase of W and C, a bonding phase of iron group metals, and a condensed phase of Zr and Nb is used as the substrate, and a coating such as TiCN, Al2O3 or TiN is formed on the surface, and the film is formed by CVD. , control the atomic ratio of Nb/(Zr+Nb) to be less than 0.38 to improve heat resistance and wear resistance.

Benefits of technology

Significantly improves the heat resistance and wear resistance of cemented carbide, extends the service life of coated tools, and enhances the stability and durability of cutting operations at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786233A_ABST
    Figure CN118786233A_ABST
Patent Text Reader

Abstract

A cemented carbide according to an undefined embodiment of the present disclosure contains: a hard phase containing W and C; a binder phase comprising one or more iron group metals; and a condensed phase containing Zr and Nb, the atomic ratio of Nb / (Zr + Nb) being less than 0.38. A coated tool of an undefined manner of the present disclosure has the cemented carbide and a coating located on the surface of the cemented carbide. A cutting tool according to an undefined embodiment of the present disclosure is provided with: a shank extending from a first end toward a second end and having a pocket on the first end side; and the coated cutter is positioned in the cutter groove.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This application claims the benefit of priority based on Japanese Patent Application No. 2022-032394 filed on March 3, 2022, and the entire disclosure of the prior application is incorporated herein by reference. Technical Field

[0003] The present invention relates to cemented carbide and a coated tool and a cutting tool using the same. Background Art

[0004] Cemented carbide containing WC (tungsten carbide) as a hard phase is used for substrates in coated tools, etc., and for cutting tools such as end mills. For example, Japanese Patent Gazette No. 5424935 (Patent Document 1) states that by dispersing a ZrO2 phase (zirconium oxide phase) on the surface of a substrate composed of cemented carbide, it is possible to suppress the peeling of the coating caused by the thermal expansion difference between the substrate and the coating. Summary of the invention

[0005] A cemented carbide according to an unrestricted embodiment of the present disclosure comprises: a hard phase comprising W and C; a binder phase comprising one or more iron group metals; and a condensed phase comprising Zr and Nb, wherein the atomic ratio Nb / (Zr+Nb) is less than 0.38.

[0006] A coated tool according to one non-limited aspect of the present disclosure includes: the above-mentioned cemented carbide; and a coating located on a surface of the cemented carbide.

[0007] A cutting tool according to one non-limited aspect of the present disclosure includes: a shank extending from a first end toward a second end and having a groove on the first end side; and the above-mentioned coated tool located in the groove. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Figure 1 This is a schematic diagram showing a cross section of a cemented carbide according to one embodiment of the present disclosure which is not limited thereto.

[0009] Figure 2 This is a perspective view showing a coated tool according to one embodiment of the present disclosure which is not limited thereto.

[0010] Figure 3 This is a cross-sectional view showing the vicinity of the surface of a coated tool according to one embodiment of the present disclosure which is not limited thereto.

[0011] Figure 4 This is a cross-sectional view showing the vicinity of the surface of a coated tool according to one embodiment of the present disclosure which is not limited thereto.

[0012] Figure 5 This is a perspective view showing a cutting tool according to one embodiment of the present disclosure which is not limited thereto. DETAILED DESCRIPTION

[0013] <Hard alloy>

[0014] Hereinafter, the unrestricted cemented carbide 1 of the present disclosure will be described in detail using the accompanying drawings. However, in the following referenced figures, for the convenience of description, only the main components required in the description of the embodiment are simplified. Therefore, the cemented carbide 1 may have any constituent components not shown in the referenced figures. In addition, the dimensions of the components in the figures do not faithfully represent the dimensions of the actual constituent components and the dimensional ratios of the components. These aspects are also the same in the coated tool and cutting tool described later.

[0015] Cemented carbide 1 can be Figure 1 As shown in the non-limiting example, the hard phase 3, the binder phase 5 and the aggregate phase 7 are included.

[0016] The hard phase 3 may contain W (tungsten) and C (carbon). In other words, the hard phase 3 may contain WC. The hard phase 3 may contain WC as a main component. The "main component" may refer to a component having the largest mass % value compared to other components.

[0017] The binding phase 5 may be composed of one or more iron group metals such as Co (cobalt) and Ni (nickel). The binding phase 5 may be composed of at least one of Co and Ni. The binding phase 5 can function as a phase that binds the adjacent hard phases 3. The binding phase 5 may be composed only of an iron group metal, and may contain some additives and / or impurities. Specifically, the binding phase 5 may contain 95% by mass or more of an iron group metal, and may contain 5% by mass or less of additives and / or impurities.

[0018] The aggregate phase 7 may also be referred to as a so-called β phase. The aggregate phase 7 can function as a phase that imparts heat resistance to the cemented carbide 1 .

[0019] Here, the condensed phase 7 may contain Zr (zirconium) and Nb (niobium). That is, the condensed phase 7 may be a phase formed by the condensation of at least Zr and Nb. In addition, the condensed phase 7 may have an atomic ratio of Nb / (Zr+Nb) less than 0.38. In the condensed phase 7, when Zr is present in a larger amount than Nb at such a ratio, the heat resistance of the cemented carbide 1 is easily improved. Therefore, the heat resistance of the cemented carbide 1 is high.

[0020] It should be noted that the lower limit of Nb / (Zr+Nb) in terms of atomic ratio may be greater than 0. Specifically, the lower limit may be 0.02. Nb is a component intentionally added for the purpose of improving heat resistance. In addition, the value of Nb / (Zr+Nb) in terms of atomic ratio may be an average value.

[0021] The aggregate phase 7 may contain Zr at a ratio of 1 to 10 atomic % (at %). In addition, the aggregate phase 7 may contain Nb at a ratio of 0.5 to 3 atomic %.

[0022] The condensed phase 7 may contain C, Ti (titanium), Co, Ta (tantalum), W, etc. in addition to Zr and Nb. The condensed phase 7 may contain C at the highest atomic ratio.

[0023] Elemental analysis when calculating atomic ratios, etc. can be performed, for example, by energy dispersive X-ray spectroscopy (EDS). Elemental analysis can be performed by cross-sectional observation using EDS attached to an electron microscope. Examples of electron microscopes include scanning electron microscopes (SEM) and transmission electron microscopes (TEM).

[0024] The aggregated phase 7 may contain the first aggregated phase 9. The first aggregated phase 9 may have an atomic ratio of Nb / (Zr+Nb) of 0.25 or less. In this case, the heat resistance of the cemented carbide 1 is easily improved.

[0025] The first condensed phase 9 may be less than 0.2 in terms of the atomic ratio Nb / (Zr+Nb). In this case, it is expected that the heat resistance will be improved. In addition, if the tool is coated, the wear resistance will be improved. It should be noted that the first condensed phase 9 may be greater than 0.05 in terms of the atomic ratio Nb / (Zr+Nb).

[0026] The condensed phase 7 may further contain a second condensed phase 11 and a third condensed phase 13. The second condensed phase 11 may have an atomic ratio of Nb / (Zr+Nb) greater than 0.3 and less than 0.34. The third condensed phase 13 may have an atomic ratio of Nb / (Zr+Nb) greater than 0.34 and less than 0.38. In these cases, the heat resistance of the cemented carbide 1 is easily improved.

[0027] The average grain size of the first condensed phase 9 may be smaller than the average grain size of the second condensed phase 11 and the average grain size of the third condensed phase 13. In this case, the heat resistance of the cemented carbide 1 is likely to be improved.

[0028] The average grain size of the third condensed phase 13 may be smaller than the average grain size of the second condensed phase 11. In this case, the heat resistance of the cemented carbide 1 is likely to be improved.

[0029] The average grain size of the second condensed phase 11 may be larger than the average grain size of the first condensed phase 9 and the average grain size of the third condensed phase 13. In this case, the heat resistance of the cemented carbide 1 is likely to be improved.

[0030] The average particle size of the first condensed phase 9 is not limited to a specific size. This also applies to the average particle size of the second condensed phase 11 and the average particle size of the third condensed phase 13. The average particle size of the first condensed phase 9 may be 0.5 to 4 μm. The average particle size of the second condensed phase 11 may be 1.5 to 5 μm. The average particle size of the third condensed phase 13 may be 1 to 4.5 μm.

[0031] The average particle size of the first condensed phase 9 can be determined by image analysis. In this case, the equivalent circle diameter can be used as the average particle size of the first condensed phase 9. The average particle size of the first condensed phase 9 can be determined by the following sequence. First, a SEM can be used to observe the cross section of the cemented carbide 1 at a magnification of 3000 to 5000 times to obtain an SEM image. At least 50 first condensed phases 9 in the SEM image can be determined and extracted. Then, the average particle size of the first condensed phase 9 can be obtained by calculating the equivalent circle diameter using the image analysis software ImageJ (1.52). The average particle size of the second condensed phase 11 and the average particle size of the third condensed phase 13 can be determined in the same order as the average particle size of the first condensed phase 9.

[0032] <Method for producing cemented carbide>

[0033] Next, a method for producing a cemented carbide according to one embodiment of the present disclosure, which is not limited thereto, will be described by taking a case where the cemented carbide 1 is produced as an example.

[0034] First, as raw material powders, WC powder, Co powder, TiC powder, ZrC powder, NbC powder, TaC powder, etc. can be prepared.

[0035] The proportion of Co powder may be 4 to 15 mass % (wt%). The proportion of TiC powder may be 0.5 to 5 mass %. The proportion of ZrC powder may be 0.2 to 5 mass %. The proportion of NbC powder may be 0.1 to 3 mass %. The proportion of TaC powder may be 0.1 to 5 mass %. The remainder may be WC powder. The proportion of ZrC powder may be set to be greater than that of NbC powder.

[0036] The average particle size of the raw material powder can be appropriately selected within the range of 0.1 to 10 μm. The average particle size of the raw material powder can be a value measured by the Microtrac method.

[0037] The prepared raw material powders can be mixed and molded to obtain a molded body. Examples of the molding method include press molding, casting molding, extrusion molding, and cold isostatic pressing.

[0038] The obtained molded body may be subjected to dewaxing treatment and then fired. The firing may be performed in a non-oxidizing atmosphere such as vacuum, argon atmosphere, and nitrogen atmosphere. The firing temperature may be 1450 to 1600° C. The firing time may be 0.5 to 3 hours.

[0039] After sintering, the hard alloy 1 can be obtained by cooling. At this time, the cooling process can be set to maintain the temperature in the range of 900 to 1400°C for 0.25 to 2 hours. If such a maintenance (maintaining temperature and holding time) is set in the cooling process, it is easy to form a condensed phase 7 in which the atomic ratio Nb / (Zr+Nb) is less than 0.38. In addition, it is easy to form a condensed phase 7 containing the first condensed phase 9, the second condensed phase 11 and the third condensed phase 13.

[0040] It should be noted that the above-mentioned manufacturing method is an example of a method for manufacturing the cemented carbide 1. Therefore, the cemented carbide 1 is of course not limited to the cemented carbide manufactured by the above-mentioned manufacturing method.

[0041] <Coated tools>

[0042] Next, the case of the above-mentioned cemented carbide 1 is taken as an example, and the Figure 2 to Figure 4 A coated tool 101 according to one embodiment of the present disclosure which is not limited thereto will be described.

[0043] The coated tool 101 can be Figure 2 to Figure 4 As shown in the non-limited example, the coated tool 101 has a cemented carbide 1 and a coating 103 located on the surface 15 of the cemented carbide 1. The coated tool 101 can have the cemented carbide 1 as a substrate. In the case where the coated tool 101 has the cemented carbide 1, the wear caused by heat is suppressed because the heat resistance of the cemented carbide 1 is high. Therefore, the wear resistance of the cemented carbide 1 (substrate) is high, and combined with the wear resistance based on the coating 103, the durability of the coated tool 101 is high.

[0044] The coating layer 103 may be located on the entire surface 15 of the cemented carbide 1 or may be located on only a portion thereof. In other words, the coating layer 103 may be located on at least a portion of the surface 15 of the cemented carbide 1 .

[0045] The coating 103 can be formed by chemical vapor deposition (CVD). In other words, the coating 103 can be a CVD film. It should be noted that the coating 103 can be a PVD film formed by physical vapor deposition (PVD).

[0046] The coating layer 103 may be a single layer structure or a structure in which a plurality of layers are stacked. Examples of the composition of the coating layer 103 include TiCN (titanium carbonitride), Al2O3 (aluminum oxide), and TiN (titanium nitride).

[0047] The coating 103 may be Figure 3 As shown in the non-limiting example, the TiCN layer 105 and the Al2O3 layer 107 are provided in this order from the cemented carbide 1. The TiCN layer 105 may be in contact with the cemented carbide 1. The Al2O3 layer 107 may be in contact with the TiCN layer 105.

[0048] The coating 103 may be Figure 4 As shown in the non-limiting example, the TiN layer 109, the TiCN layer 105 and the Al2O3 layer 107 are provided in this order from the cemented carbide 1. The TiN layer 109 may be in contact with the cemented carbide 1. The TiCN layer 105 may be in contact with the TiN layer 109. The Al2O3 layer 107 may be in contact with the TiCN layer 105.

[0049] The coating 103 is not limited to a specific thickness. For example, the thickness of the TiCN layer 105 can be set to about 1 to 15 μm. The thickness of the Al2O3 layer 107 can be set to about 1 to 15 μm. The thickness of the TiN layer 109 can be set to about 0.1 to 5 μm. The thickness of the coating 103 can be measured by cross-sectional observation using an electron microscope. In addition, the thickness of the coating 103 can be an average value. For example, the thickness can be measured at any position of each layer at a width range of more than 10 μm at intervals of 1 μm at more than 10 measurement points, and the average value is calculated.

[0050] exist Figure 2 , a cutting insert is shown as a non-limiting example of the coated tool 101. It should be noted that the coated tool 101 is not limited to the cutting insert.

[0051] The coated tool 101 may include a first surface 111 (upper surface), a second surface 113 (side surface) adjacent to the first surface 111 , and a cutting edge 115 located at least partially at a ridgeline between the first surface 111 and the second surface 113 .

[0052] The first surface 111 may be a rake face. The first surface 111 may be the entire rake face, or a portion thereof may be the rake face. For example, a region along the cutting edge 115 of the first surface 111 may be the rake face.

[0053] The second surface 113 may be a flank surface. The entire surface of the second surface 113 may be a flank surface, or a portion of the second surface 113 may be a flank surface. For example, a region along the cutting edge 115 of the second surface 113 may be a flank surface.

[0054] The cutting edge 115 may be located at a part of the ridge portion or may be located at the entire ridge portion. The cutting edge 115 can be used for cutting a workpiece.

[0055] The coated tool 101 may have a through hole 117. The through hole 117 can be used to install a fixing screw or a clamping member when the coated tool 101 is held in the tool holder. The through hole 117 can be formed from the first surface 111 to the surface (lower surface) on the opposite side of the first surface 111, and can also be opened on these surfaces. It should be noted that there is no problem even if the through hole 117 is opened in the mutually opposing regions of the second surface 113.

[0056] The coated tool 101 may be in the shape of a quadrilateral plate. It should be noted that the shape of the coated tool 101 is not limited to the quadrilateral plate shape. For example, the first surface 111 may be in the shape of a triangle, a pentagon, a hexagon or a circle.

[0057] The coated tool 101 is not limited to a specific size. For example, the length of one side of the first surface 111 can be set to about 3 to 20 mm. In addition, the height from the first surface 111 to the surface (lower surface) located on the opposite side of the first surface 111 can be set to about 5 to 20 mm.

[0058] <Method for manufacturing coated cutting tools>

[0059] Next, a method for manufacturing a coated tool according to one embodiment of the present disclosure, which is not limited thereto, will be described by taking a case where the coated tool 101 is manufactured as an example.

[0060] The coating 103 can be formed on the surface 15 of the cemented carbide 1 by a CVD method to obtain the coated tool 101 .

[0061] The TiCN layer 105 can be formed as follows. First, as a reaction gas composition, a mixed gas composed of 0.1 to 10 volume % titanium tetrachloride (TiCl4) gas, 10 to 60 volume % nitrogen (N2) gas, 0.1 to 15 volume % methane (CH4) gas, and the remainder hydrogen (H2) gas can be adjusted. Then, the mixed gas can be introduced into the furnace, the temperature is set to 800 to 1100°C, and the pressure is set to 5 to 30 kPa to form the TiCN layer 105.

[0062] The Al2O3 layer 107 can be formed as follows. First, as a reaction gas composition, a mixed gas consisting of 0.5 to 5 volume % of aluminum chloride (AlCl3) gas, 0.5 to 3.5 volume % of hydrogen chloride (HCl) gas, 0.5 to 5 volume % of carbon dioxide (CO2) gas, 0.5 to 5 volume % of hydrogen sulfide (H2S) gas below 0.5 volume %, and the remainder of hydrogen (H2) gas can be adjusted. Then, the mixed gas can be introduced into the furnace, the temperature can be set to 930 to 1010°C, and the pressure can be set to 5 to 10 kPa to form the Al2O3 layer 107.

[0063] The TiN layer 109 can be formed as follows. First, as a reaction gas composition, a mixed gas composed of 0.1 to 10 volume % titanium tetrachloride (TiCl4) gas, 10 to 60 volume % nitrogen (N2) gas, and the remainder hydrogen (H2) gas can be adjusted. Then, the mixed gas can be introduced into the furnace, the temperature can be set to 800 to 1010°C, and the pressure can be set to 10 to 85 kPa to form the TiN layer 109.

[0064] It should be noted that the above-mentioned manufacturing method is an example of a method for manufacturing the coated tool 101. Therefore, the coated tool 101 is of course not limited to the coated tool manufactured by the above-mentioned manufacturing method.

[0065] <Cutting tools>

[0066] Next, the case of having the above-mentioned coated tool 101 is cited as an example, using Figure 5 A cutting tool 201 according to one embodiment of the present disclosure which is not limited thereto will be described.

[0067] The cutting tool 201 may be Figure 5 As shown in the non-limiting example, the cutting tool 201 includes: a tool holder 203 extending from a first end 203a toward a second end 203b and having a tool groove 205 on the first end 203a side; and a coated tool 101 located in the tool groove 205. When the cutting tool 201 includes the coated tool 101, stable cutting can be performed due to the high durability of the coated tool 101.

[0068] The knife groove 205 may be a portion for mounting the coated tool 101. The knife groove 205 may be open on the outer peripheral surface of the tool handle 203 and the end surface on the first end 203a side.

[0069] The coated tool 101 can be mounted on the knife groove 205 in a manner that the cutting edge 115 protrudes outward from the tool handle 203. In addition, the coated tool 101 can be mounted on the knife groove 205 by a fixing screw 207. That is, the fixing screw 207 can be inserted into the through hole 117 of the coated tool 101, and the front end of the fixing screw 207 can be inserted into the threaded hole formed in the knife groove 205 and screwed with the threaded portion, thereby mounting the coated tool 101 on the knife groove 205. At this time, the lower surface of the coated tool 101 can be in direct contact with the knife groove 205, and a sheet material can be clamped between the coated tool 101 and the knife groove 205.

[0070] Examples of the material of the handle 203 include steel and cast iron. When the material of the handle 203 is steel, the handle 203 has high toughness.

[0071] exist Figure 5 In the example shown, a cutting tool 201 used for so-called turning processing is illustrated. As turning processing, for example, inner diameter processing, outer diameter processing, and grooving processing can be cited. It should be noted that the use of the cutting tool 201 is not limited to turning processing. For example, there is no problem even if the cutting tool 201 is used for milling processing.

[0072] As mentioned above, although the cemented carbide 1, the coated tool 101, and the cutting tool 201 which are one embodiment not limited to this disclosure are illustrated, this disclosure is not limited to the above-mentioned embodiment, and it is obvious that any embodiment is possible as long as it does not deviate from the gist of this disclosure.

[0073] For example, in the above-mentioned non-limiting embodiment, the case where the cemented carbide 1 is used for the coated tool 101 and the cutting tool 201 is described as an example, but the cemented carbide 1 can also be applied to other uses. As other uses, for example, sliding parts, wear-resistant parts such as molds, tools such as excavators and cutters, and impact-resistant parts can be cited.

[0074] Hereinafter, the present disclosure will be described in detail with reference to Examples, but the present disclosure is not limited to the following Examples.

[0075] Example

[0076] [Sample No. 1 to 4]

[0077] <Production of cemented carbide>

[0078] First, WC powder with an average particle size of 3 μm, Co powder with an average particle size of 1.5 μm, TiC powder with an average particle size of 1 μm, ZrC powder with an average particle size of 1 μm, NbC powder with an average particle size of 1 μm, and TaC powder with an average particle size of 1 μm were prepared as raw material powders. The average particle size of the raw material powders was measured by the Microtrac method.

[0079] Next, the raw material powders were mixed so that the composition of the condensed phase in the sintered body became the composition shown in Table 1, and the shaped body was obtained by pressing into a cutting tool shape (CNMG120408). After the obtained shaped body was dewaxed, it was sintered at a temperature of 1450 to 1600° C. for 0.5 to 2 hours. Then, after sintering, it was cooled under the cooling conditions shown in Table 2 to obtain a cemented carbide composed of a sintered body containing a condensed phase of the composition shown in Table 1.

[0080] Elemental analysis was performed by EDS. Specifically, it was performed by cross-sectional observation using EDS attached to SEM. Three arbitrary locations were measured at a magnification of 5000 to 20000 times, and the average value was calculated. In addition, the atomic ratio Nb / (Zr+Nb) was calculated based on the average value.

[0081] It should be noted that the results of the EDS measurement show that the obtained cemented carbides all contain a hard phase containing W and C and a binder phase composed of a ferrous metal (Co) as main components. In addition, Samples No. 3 to 4 contain condensed phases whose values ​​of Nb / (Zr+Nb) in terms of atomic ratio are different from the numerical range of the first to third condensed phases, but for convenience, they are recorded in the columns of the first to third condensed phases in Tables 1 and 2.

[0082] <Evaluation>

[0083] The obtained cemented carbide was evaluated for cutting. Specifically, a TiN layer with a thickness of 1 μm, a TiCN layer with a thickness of 10 μm, and an Al2O3 layer with a thickness of 5 μm were formed from the cemented carbide (substrate) by CVD to make a coated tool, and then the cutting evaluation was performed under the following conditions. It should be noted that the thickness of each layer is an average value.

[0084] Processing method: Turning

[0085] Cutting speed: 300m / min

[0086] Feed: 0.3mm / rev

[0087] Cutting depth: 2mm

[0088] Workpiece: SCM435φ200 round bar

[0089] Processing status: WET

[0090] The evaluation results are shown in Table 2. In addition, the "wear amount of the flank face" in the evaluation results of Table 2 indicates the wear amount on the flank face of the cutting edge when the cutting process is performed.

[0091] [Table 1]

[0092]

[0093] [Table 2]

[0094]

[0095] Compared with samples No. 3 and 4, samples No. 1 and 2 have significantly improved stability.

[0096] The results of measuring the average particle sizes of the first to third aggregated phases in Samples Nos. 1 and 2 by the above-mentioned image analysis showed that the average particle sizes of the first to third aggregated phases had a relationship of second aggregated phase>third aggregated phase>first aggregated phase.

[0097] Description of reference numerals:

[0098] 1. Carbide

[0099] 3 Hard phase

[0100] 5. Adhesive Phase

[0101] 7 Condensed phase

[0102] 9 First condensed phase

[0103] 11 Second condensed phase

[0104] 13 The third condensed phase

[0105] 15 Surface

[0106] 101 Coated Tools

[0107] 103 coating

[0108] 105TiCN layer

[0109] 107Al2O3 layer

[0110] 109TiN layer

[0111] 111 First surface (upper surface)

[0112] 113 Second side (side)

[0113] 115 cutting edge

[0114] 117 through holes

[0115] 201 cutting tools

[0116] 203 handle

[0117] 203a First End

[0118] 203b Second end

[0119] 205 knife groove

[0120] 207 fixing screws.

Claims

1. A cemented carbide, in, The cemented carbide contains: a hard phase, which contains W and C; a binder phase composed of one or more iron group metals; and The condensed phase contains Zr and Nb, and the atomic ratio Nb / (Zr+Nb) is less than 0.

38.

2. The cemented carbide according to claim 1, in, The aggregated phase includes a first aggregated phase, and the first aggregated phase has an atomic ratio of Nb / (Zr+Nb) of 0.25 or less.

3. The cemented carbide according to claim 2, in, The coacervate phase further comprises: A second condensed phase having an atomic ratio of Nb / (Zr+Nb) greater than 0.3 and not more than 0.34; and The third condensed phase has an atomic ratio of Nb / (Zr+Nb) greater than 0.34 and less than 0.

38.

4. The cemented carbide according to claim 3, in, The average particle size of the first coacervate phase is smaller than the average particle size of the second coacervate phase and the average particle size of the third coacervate phase.

5. The cemented carbide according to claim 3 or 4, in, The average particle size of the third coacervate phase is smaller than the average particle size of the second coacervate phase.

6. A coated tool, in, The coated tool has: The cemented carbide according to any one of claims 1 to 5; and The coating is located on the surface of the cemented carbide.

7. The coated tool according to claim 6, in, The coating has a TiCN layer and an Al layer in sequence starting from the cemented carbide. 2 O 3 layer.

8. The coated tool according to claim 6, in, The coating layer has a TiN layer, a TiCN layer and an Al layer in sequence from the cemented carbide. 2 O 3 layer.

9. A cutting tool, in, The cutting tool has: a knife handle extending from a first end toward a second end and having a knife groove on a side of the first end; and The coated tool according to any one of claims 6 to 8, which is located in the tool groove.