Method for producing optical layer system and optical layer system produced using method

By using hydrogenated amorphous silicon or hydrogenated germanium of the same material to deposit the optical layer system, and using processes such as sputtering to adjust the refractive index and extinction coefficient, the problems of long flushing time and complex processes in the existing technology are solved, and high efficiency and high efficiency are achieved. Simple production of optical layer systems suitable for manufacturing high-volume, high-quality products.

CN118786241AInactive Publication Date: 2024-10-15FHR ANLAGENBAU GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092951.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-01
Filing Date
2022-06-15
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing optical filters have long rinsing times and complex process flows during the manufacturing process, resulting in low production efficiency and high costs, and alternate deposition between materials requires different coating sources and process gases, resulting in long process times. .

Method used

The same material is used to deposit hydrogenated amorphous silicon (a-Si:H) or hydrogenated germanium (Ge:H). The refractive index and extinction coefficient of each layer are adjusted by controlling the sputtering process parameters, simplifying the process and reducing flushing time. , using methods such as sputtering, chemical vapor deposition or electron beam evaporation processes to achieve efficient production.

Benefits of technology

It achieves fast and simple production of optical layer systems, reduces process time and cost, ensures consistency and high efficiency of layer characteristics, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118786241A_ABST
    Figure CN118786241A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing an optical layer system and to an optical layer system comprising a plurality of layers arranged on a substrate wherein a portion of the layers has a high refractive index nH and another portion of the layers has a low refractive index nL and a further portion of the layers has a medium refractive index nM wherein nH > nM > nL, and wherein layers having different refractive indices are alternately stacked. The aim of the invention is to provide a method that makes it possible for the layers of deposits not to have a long rinsing time between them, in which an optical layer system can be achieved in a simple, comparatively short process time, quality-consistent, and quantity manner by depositing the layers of the optical layer system from the same material onto a substrate by means of a selected coating method, the material is amorphous silicon hydride (a-Si: H) or germanium hydride (Ge: H), wherein the refractive index and extinction coefficient of each of the plurality of layers of the layer system are adjusted by controlling the process parameters of the selected coating method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing an optical layer system composed of a plurality of layers.

[0002] The invention further relates to an optical layer system which is produced by the method according to the invention and comprises a plurality of layers arranged on a substrate, a portion of the layers having a high refractive index n H and the other part of the layer has a low refractive index n L And there is also a part of the layer with a medium refractive index n M , where n H >n M >n L , and layers with different refractive indexes are alternately stacked. Background Art

[0003] Optical layer systems, in particular optical filters, such as bandpass filters for time-of-flight (ToF) spectroscopy for facial or gesture recognition or lidar for optical distance and speed measurement, are made of two different optical materials for the near infrared (NIR) or infrared (IR) range. They are made, for example, of a-Si:H as a high refractive index material and SiO as a low refractive index material. 2 composition.

[0004] In a typical gesture recognition system, a light source emits near-infrared light toward the user. An image sensor captures the emitted light reflected from the user to provide a 3D image of the user. A processing system then analyzes the 3D image to recognize the gesture made by the user.

[0005] Optical filters, in particular bandpass filters, are used to transmit emitted light to an image sensor while substantially blocking ambient light. Optical filters are therefore used to shield ambient light. Therefore, there is a need for an optical filter with a narrow passband range in the near infrared wavelength range (i.e., 800nm ​​to 1100nm). In addition, the optical filter must have a high transmission level / degree within the passband range and a high stopband or stopband outside the passband range, wherein the transmission in the stopband is ideally close to zero.

[0006] Conventionally, an optical filter comprises two bandpass filters arranged on opposite surfaces of a substrate. The passband ranges of the bandpass filters are coordinated with each other so that the passband range of the bandpass filter on the back side of the substrate envelopes the passband range of the filter on the front side of the substrate. At the same time, the passband ranges of the filters are coordinated with each other so as to produce an anti-reflection effect. Therefore, the bandpass filter on the back side of the substrate blocks wavelengths outside the passband range of the bandpass filter on the front side of the substrate. Each filter consists of alternating stacks of high refractive index layers and low refractive index layers. Usually, different oxides are used for the high refractive index layers and the low refractive index layers, such as titanium dioxide (TiO 2), niobium pentoxide (Nb 2 O 5 ), Tantalum pentoxide (Ta 2 O 5 ) or silicon dioxide (SiO 2 ).

[0007] US 9945995 B2 discloses an optical filter whose passband range at least partially overlaps with the wavelength range of 800nm ​​to 1100nm. The optical filter comprises a filter stack, which is composed of hydrogenated silicon layers as high refractive index layers and low refractive index layers stacked alternately. Each hydrogenated silicon layer has a refractive index greater than 3 in the wavelength range of 800nm ​​to 1100nm, and has an extinction coefficient less than 0.0005 in the wavelength range of 800nm ​​to 1100nm. The lower refractive index material is a dielectric material, usually an oxide. A suitable lower refractive index material is silicon dioxide (SiO 2 ), aluminum oxide (Al 2 O 3 ), titanium dioxide (TiO 2 ), niobium pentoxide (Nb 2 O 5 ), Tantalum pentoxide (Ta 2 O 5 ) and mixtures thereof, i.e. mixed oxides.

[0008] An optical interference filter with improved transmittance in the passband range of the filter is also known from US 9989684 B2. The disclosed interference filter comprises a stack of multiple layers, at least one layer of which consists of hydrogenated amorphous silicon with a high refractive index and at least one layer of one or more dielectric materials having a refractive index lower than that of hydrogenated amorphous silicon.

[0009] In order to improve the performance of optical filters, for example in gesture recognition systems, it is necessary to reduce the number of layers, the total coating thickness and the wavelength shift as a function of the angle of incidence (AOI - angle of incidence). In addition, there should be a minimum transmittance in the stopband region outside the passband range. For the purposes of the present invention, the wavelength shift is understood to mean the shift of the passband of the filter, which should be as small as possible so that almost the same filter characteristics are presented at different viewing angles of the filter. One way to improve this is to use a material with a higher refractive index than conventional oxides in the wavelength range of interest for the high refractive index layer, such as disclosed in US 9945995 B2. In addition to the higher refractive index, the material must also have a lower extinction coefficient in the wavelength range of interest to provide a high level of transmission in the passband range. However, to date, different materials have been used for layers with different refractive indices.

[0010] The main disadvantage of using different materials for such optical filters is that they are usually deposited on the substrate within the same coating system. Different coating sources and coating processes need to be used, where each coating source uses a different process gas. This requires long flushing processes when changing the coating source and thus the process gas, which leads to very long processing times. The method of producing high-quality optical interference filters or optical layer systems with many different layers and layer materials is also complex and time-consuming. Summary of the invention

[0011] It is therefore an object of the present invention to provide a method for producing an optical layer system which overcomes the disadvantages of the prior art, such as long rinse times between the deposition of the individual layers. By means of the method, the optical layer system can be produced simply, in particular the process time should be as short as possible, so that a high quantity of end products with a consistent quality can be achieved.

[0012] A further object of the present invention is to provide an optical layer system which has optimal layer properties for its field of application and which can be produced in a highly reproducible and efficient manner.

[0013] This object is achieved by a method for producing an optical layer system consisting of a plurality of layers according to independent claim 1 .

[0014] In a method for manufacturing an optical layer system consisting of a plurality of layers according to the present invention, the layers of the optical layer system are deposited onto a substrate from the same material, which is hydrogenated amorphous silicon (a-Si:H) or hydrogenated germanium (Ge:H), by means of a selected coating method, wherein the refractive index and extinction coefficient of each of the plurality of layers of the layer system are adjusted by controlling the process parameters of the selected coating method.

[0015] It is particularly advantageous that in the method for producing an optical layer system according to the invention, regardless of the coating method, only a single material, i.e. a-Si:H:x or Ge:H:x, is deposited and the optical properties, such as the refractive index and the extinction coefficient of each layer, can only be set by controlling a typical process parameter or a plurality of typical process parameters of the selected coating method, x may represent another process gas, such as nitrogen (N 2 ) or chlorine (Cl 2 ). This means that the manufacturing method is very simple, shorter and therefore more cost-effective than existing technologies due to the elimination of the need for flushing processes between different layers of materials and process gases.

[0016] In a configuration of the method according to the invention, the coating method is a sputtering process, wherein the sputtering process is a process of depositing a coating layer by argon (Ar) and / or krypton (Kr) and / or helium (He) and / or xenon (Xe) and hydrogen (H 2), or the sputtering of silicon is carried out using a reactive gas mixture of Ar, Kr, He and / or Xe, and the layers of the layer system are hydrogenated to form a-Si:H or Ge:H by means of a plasma and / or ion source, or the sputtering process is carried out as a combination of reactive sputtering and the plasma and / or ion source used, wherein the refractive index and the extinction coefficient of each individual a-Si:H:x or Ge:H:x layer of the layer system are adjusted by the ratio of Ar, Kr, He and / or Xe to hydrogen, x representing a further layer component which can be present in embodiments of the method but does not necessarily have to be present. This applies to all selectable coating processes.

[0017] If sputtering technology is chosen as the coating process, there are various production options for producing a-Si:H or Ge:H. One variant is to carry out the sputtering process reactively, i.e. using a reactive gas mixture, preferably consisting of argon and hydrogen. For other layer compositions, such as a-Si:H:N, nitrogen or oxygen can also be used as reactive gas for the sputtering process. Using nitrogen (N) or oxygen (O 2 ) has the advantage that, due to the larger ionic or atomic radius relative to hydrogen, the layer stress of the deposited layer can be corrected in the direction of compressive stress. As a result, the tensile stress in the a-Si:H or Ge:H layer can be reduced or corrected.

[0018] In another variant, the sputtering process can be carried out with argon and / or krypton and / or helium and / or xenon, so that only a subnanometer thick silicon or germanium layer is deposited by sputtering, which is hydrogenated or nitrated or oxidized or oxynitrated or hydronitrated in a post-treatment step with an ion and / or plasma source. These two process steps are repeated iteratively until the desired layer thickness is reached. In the post-treatment step, the substrate with the metal sputtered layer is passed through a plasma generated by a plasma and / or ion source. The source can be, for example, an ICP (inductively coupled plasma) source.

[0019] The third variant represents a combination of the two variants mentioned above. The reactive gas is used both for the sputtering process for depositing sub-nanometer thick layers and for post-treatment using a plasma and / or ion source. The final stoichiometry and structure of the a-Si:H:x or Ge:H:x layer are set by selecting the gas flow, the proportion of argon added to the reactive gas in the sputtering source or plasma and / or ion source, the power of the sputtering source or plasma and / or ion source and the temperature of the surface / substrate to be coated. These then determine the optically relevant variables, such as the refractive index and extinction coefficient of each individual layer of the optical layer system.

[0020] Prior to the production of the layers, the relationship between the optical properties of the high, medium and low refractive index layers and the process variables of the sputtering process is determined experimentally. Individual process steps in the deposition of the optical layer system are relevant to these studies. An important control variable in the production of a-Si:H:x or Ge:H:x layers is the ratio of hydrogen to the reaction gas, for example argon, wherein the higher the proportion of hydrogen in the reaction gas, the lower the material density and thus the refractive index. The set ratio of argon to hydrogen is set to a value of 1:2 to 5:1, in particular in the range of 1:3 to 4:1. The ratio of the gas mixtures to one another is selected so that the refractive index can be set within the range relevant to the filter, so that the refractive index can be as high as possible and the extinction coefficient can be as low as possible for the cavity of the filter to be produced. Based on this, the refractive index of the high refractive index layer of the filter stack is set higher, wherein the associated loss of the extinction coefficient is acceptable here. Likewise, the refractive index of the low refractive index layer of the filter stack is set as low as possible and the smallest possible extinction coefficient is observed.

[0021] The deposition of a-Si:H:N is an example of a filter stack layer to be deposited. Likewise, layers formed of a-Si:H:N:Cl, a-(Si,Ge):H, a-(Si,Ge):H:N and / or a-(Si,Ge):H:N:Cl can be generated using the method according to the invention. Other combinations of hydrogenated silicon or germanium with reactive gases are possible and are not limited to the aforementioned combinations.

[0022] In another embodiment of the method according to the invention, the reactive gas mixture is argon and nitrogen N 2 or argon and oxygen O 2 The choice of the reactive gas mixture depends on the composition of the layer to be deposited. This has the advantage that, due to the larger ionic or atomic radius compared to hydrogen, the layer stresses can be corrected in the direction of compressive stresses. This makes it possible to reduce or correct tensile stresses in a-Si:H or Ge:H layers.

[0023] In another variant of the method according to the invention, the coating method is a chemical vapor deposition process (chemical vapor deposition (CVD) process), wherein the CVD process is carried out by plasma assistance, by catalysis or by thermal treatment by means of an evaporator unit and a plasma source, wherein the refractive index and the extinction coefficient of each a-Si:H or Ge:H layer of the layer system are adjusted by gas flow control by the ratio of silane or germane to hydrogen or by the power of the evaporator unit and the plasma source. Gas flow control means setting the absolute gas flow of silane or germane gas or hydrogen, or keeping one of the silane or germane gas or hydrogen constant and adjusting the other gas, or preparing a gas mixture of the two gases. Thus, the stoichiometry of the individual filter layers can be adjusted by the gas flow of silane gas or germane gas and hydrogen and their ratio to one another (partial gas flow) in the gas mixture of the plasma source or by the power of the evaporator unit and / or the plasma source.

[0024] If chemical vapor deposition (CVD) is chosen as the coating process, different variants of CVD technology such as plasma-assisted CVD (PECVD), catalytic or thermal CVD can be used to produce the a-Si:H:x or Ge:H:x layers. The optical properties of the deposited a-Si:H:x or Ge:H:x layers of the layer system are adjusted by different ratios of the reactive gases to one another. Specifically, the H 2 The ratio of process gas to silane or germane is determined in advance by experiments for different layers and the desired layer properties. These process variables are then used to create the optical layer system.

[0025] By adding nitrogen as a third reactive gas, the coating method can also be used to produce a-Si:H:N layers. It can also generate a-Si:H:N:Cl, a-(Si,Ge):H, a-(Si,Ge):H:N and / or a-(Si,Ge):H:N:Cl layers by adding more process gases or using germanium instead of silicon. Other combinations of hydrogenated silicon or germanium with reactive gases are possible and are not limited to the aforementioned combinations.

[0026] To improve the layer properties, the layer or the entire optical layer system can be heat treated in vacuum or argon atmosphere during the coating process. Typical temperatures for post-treatment annealing steps are 100-370°C, preferably 200-285°C, for 1 to 60 minutes, preferably 10 minutes.

[0027] In a thermal CVD process, a-Si:H:x or Ge:H:x layers of an optical layer system with different stoichiometries and optical properties are deposited using a silicon evaporator unit in combination with a plasma source (auxiliary source), wherein the plasma source is operated with a mixture of argon and hydrogen. In order to produce nitrides, oxides, oxynitrides or hydronitrides, the corresponding gases can also be mixed in the process. The refractive index and extinction coefficient of the individual layers of the optical layer system deposited using the thermal CVD process are adjusted by adjusting the absolute gas flow and the ratio determined before the deposition of the corresponding gas mixture partial gas flow in the ion source (e.g. silane, germane, hydrogen, etc.) and the power of the evaporator unit and the plasma source. This means that the stoichiometry can be set for each layer, so that the optical behavior can be controlled. Typically, the temperature of the substrate on which the layers are deposited is 100°C-300°C, preferably 140°C-240°C.

[0028] In preliminary tests, the optimum process parameters for the layers to be deposited with a high, low or medium refractive index are determined for a corresponding arrangement of the evaporator, the substrate to be coated and the plasma source. This known data can then be used to deposit the layers of the optical layer system.

[0029] In another further embodiment of the method according to the invention, the coating method is an electron beam evaporation process in combination with an ion source, wherein the refractive index and the extinction coefficient of each a-Si:H:x or Ge:H:x layer of the layer system are adjusted by setting the absolute gas flow and / or the ratio of the partial gas flows in the gas mixture of the ion source and the power of the evaporator unit and / or the ion source. The absolute gas flow is understood to mean the ratio of the doping gas, for example hydrogen (H 2 ) and / or nitrogen (N 2 ) and / or chlorine (Cl 2 ) and / or the total gas flow of a mixture of these doping gases. The individual doping gases can also be adjusted in partial gas flows.

[0030] If an evaporation process is chosen as a coating method for depositing a-Si:H:x or Ge:H:x layers with different stoichiometries and optical properties, a silicon or germanium evaporator unit is required in combination with an ion source (auxiliary source), wherein the ion source is operated with a mixture of argon and hydrogen. The corresponding gas mixtures can also be used to produce nitrides, oxides, oxynitrides or hydronitrides. The refractive index and extinction coefficient of each a-Si:H:x or Ge:H:x layer of the optical layer system are adjusted by adjusting the absolute gas flow and / or the ratio of the partial gas flows in the corresponding gas mixture in the ion source and the power of the evaporator and / or ion source. This means that the stoichiometry can be set for each layer and thus the optical behavior can be controlled. Typically the target substrate temperature is 100°C-300°C, preferably 140°C-240°C.

[0031] In preliminary tests, the optimum process parameters for layers with high, low or medium refractive indices are determined for a corresponding arrangement of evaporator, substrate and ion source. This known data can then be used to deposit the layers of the optical layer system.

[0032] In one embodiment of the method according to the invention, the optimal process parameters of the selected coating method for setting a defined / desired refractive index and extinction coefficient for each a-Si:H:x or Ge:H:x layer of the layer system are determined by preliminary tests or simulations.

[0033] The object of the invention is also achieved by an optical layer system according to independent claim 8 .

[0034] In an optical layer system according to the present invention produced using the method according to any one of claims 1 to 7, the multiple layers are formed of the same material, wherein the high, medium and low refractive index layers differ only in the stoichiometry of their doping gases, and wherein the optical properties of the high refractive index layer, the medium refractive index layer and the low refractive index layer can be adjusted by adjusting the stoichiometry of the doping gas using a process control device.

[0035] In a variant of the optical layer system according to the invention, the layer system has a medium refractive index n My two or more layers of, where y is an integer greater than zero and n H >n M1 ≥n M2 ≥...≥n My >n L That is, the layer system may include a plurality of layers with a medium refractive index, wherein the medium refractive index layer has a different refractive index between the high refractive index layer and the low refractive index layer relative to the high refractive index layer and the low refractive index layer. The medium refractive index layers may have partially the same and / or different refractive indices.

[0036] Thus, the layer system according to the invention can be formed from layers having only a high or low refractive index. The layers of the layer system can also have a high, medium and low refractive index, or the layer system can be formed from layers having a high refractive index layer, more than one medium refractive index layer and a low refractive index layer, wherein the refractive index of the medium refractive index layers can be partially identical or different.

[0037] Using the same chemical elements in all layers of an optical layer system has the advantage that no lengthy rinse-out processes are required between the individual layer deposition steps, since there is no need to switch between different coating materials. This means that process times are significantly shortened and large-scale production is possible.

[0038] In a preferred variant of the optical layer system according to the invention, the same material is hydrogenated amorphous silicon (a-Si:H) or hydrogenated germanium (Ge:H) and the doping gas is hydrogen (H 2 ).

[0039] Hydrogenated amorphous silicon has the significant advantage that the refractive index can be tuned over a wide range depending on the stoichiometry of the hydrogen incorporated. The use of hydrogenated silicon (Si:H) as a high refractive index layer in optical filters is described by Lairson et al. in an article entitled "Reduce Angular Shift Infrared Bandpass Filter Coatings" (SPIE Conference Proceedings, 2007, Vol. 6545, pp. 65451C-1-65451C-5) and by Gibbons et al. in an article entitled "Development and Implementation of a Reactive Sputtering Deposition Process for Hydrogenated Amorphous Silicon" (Proceedings of the Annual Technical Conference of the Society of Vacuum Coaters, 2007, Vol. 50, pp. 327-330).

[0040] In a preferred variant of the optical layer system according to the invention, the optical layer system is designed as a bandpass filter.

[0041] Preferably, the bandpass filter composed of a layer sequence of high, medium and / or low refractive index layers has a wavelength range of 800 nm to 1100 nm: for a high refractive index layer made of a-Si:H, the refractive index n H =3.35 to 3.8, extinction coefficient k<0.001, refractive index n of medium refractive index layer M =3.0 to 3.6, k<0.001, the refractive index of the low refractive index layer n L =2.5 to 3.3, k<0.001.

[0042] In another preferred variant, the bandpass filter composed of a layer sequence of high, medium and / or low refractive index layers has a wavelength range of 800 nm to 1100 nm: for a high refractive index layer made of a-Si:H:x, the refractive index n H =3.6 to 3.8, extinction coefficient k<0.0001, the refractive index of the medium refractive index layer is n M =3.2 to 3.3, k<0.0001, the refractive index of the low refractive index layer is n L =3.0 to 3.1, k<0.0001.

[0043] If the optical layer system according to the invention is designed as a bandpass filter, the optical bandpass filter preferably comprises at least two layers having a refractive index n M or L and a medium or low refractive index cavity layer with a corresponding thickness of 10 nm to 3000 nm, and at least 5 layer stacks, each layer stack consisting of alternating low refractive index and high refractive index layers, with a refractive index of n L or H , with thicknesses ranging from 5 to 200 nm respectively.

[0044] The high, medium or low refractive index layers each form a cavity in the bandpass filter, i.e. a region where constructive interference of the incident radiation occurs, thereby creating a high transmission region of the optical filter. The transmittance and the passband width of the filter can be precisely adjusted by the number of cavities formed in the optical filter. By selecting the refractive index in combination with the layer thickness of the cavity, the wavelength shift of the passband of the optical bandpass filter can be reduced. That is, when the incident angle of the incident radiation is different, almost the same filter characteristics are presented.

[0045] In addition to the cavity, there are layer stacks in the layer system, which act as mirror layers and form the so-called filter stop band. The more layer stacks with appropriate thickness are present in the optical bandpass filter, the better the incident radiation in this area is reduced by means of destructive interference.

[0046] In another variant of the optical layer system, in addition to the high refractive index layer made of a-Si:H:x or a-Ge-H:x and the low refractive index layer made of a-Si:H:x or a-Ge-H:x, the optical layer system also comprises a layer made of Si 3 N 4 or SiO 2 This layer system has the advantage that the spectrum of possible refractive indices is expanded, especially in SiO 2 The case is extended to low refractive index, SiO 2 The refractive index is 1.4 to 1.47 in the wavelength range above 800 nm. 3 N 4 In the case of a-Si:H and SiO 2 In comparison, Si represents a material with a medium refractive index. 3 N 4 With a refractive index of 2 to 2.1 in the wavelength range above 800 nm, there is the possibility that the optical parameters of the filter can be adjusted more precisely.

[0047] In a variation of the optical layer system, the optical layer system is designed as a comb filter, wherein a refractive index gradient can be formed on a plurality of layers, and the refractive index gradient can be adjusted for each of the plurality of layers by adjusting the stoichiometry of one or more doping gases by a process control device.

[0048] Due to this process, this preferred variant forms a so-called quasi-Rugate filter within each mirror system, wherein a mirror system in the sense of the present invention is understood to mean the construction of an interference filter consisting of high, medium and / or low refractive index layers and the formed cavity. A comb filter is a dielectric mirror that selectively reflects light in a specific wavelength range. This effect is achieved by a periodic, continuous or quasi-discrete change of the refractive index depending on the thickness of the mirror. Light of a specific wavelength that cannot be transmitted in the comb filter is reflected. A special challenge is to achieve a continuous or quasi-discrete refractive index distribution here. This is set by the chemical composition of the multiple filter layers as a function of the layer thickness. This can be achieved by continuously changing the gas composition during the deposition process of the individual filter layers, thereby using a dynamic process control device to adjust the stoichiometry of the doping gas in the filter material to be deposited and thus form different refractive indices.

[0049] In a further variant of the optical layer system, the optical layer system is designed as an optical interference filter.

[0050] The optical interference filter preferably has a transmission range of 420 nm to 2800 nm, preferably 800 nm to 1100 nm. The width of the passband is preferably 10 to 50 nm at 50% transmittance. The slope between 10% and 90% transmittance is preferably between 8 and 20 nm. In the range of 400 to 910 nm and in the range of 970 to 1100 nm, the transmittance of the stopband is preferably less than 1% transmittance, preferably less than 0.1% transmittance, but better still less than 0.01% transmittance.

[0051] These wavelength ranges of the passband range and the stopband are determined by the thickness of the filter layers. In particular, the width of the passband range is set by the number of cavities together with their refractive index and their layer thickness.

[0052] The final design of an optical filter depends on the requirements, which are determined by the subsequent application, for example in a sensor. This places certain demands on the passband range and the stopband. These target values ​​can be determined from the large number of layers of the optical layer system using an optical model to determine the layer stacking sequence. Thus, the thickness of the individual layers, the number, arrangement and thickness of the mirror layers and cavities determine the optical behavior of the filter.

[0053] The near-infrared range of 800 to 1100 nm is of particular interest for filter applications in sensors that use the time-of-flight method (time of flight) to determine distances and thus generate three-dimensional image information. This plays an important role in modern future-oriented technologies, such as LIDAR (Light Detection and Ranging) technology required for autonomous driving, or in human-machine interaction, such as the recognition of gestures or faces by portable end devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] The present invention will be explained in more detail below using exemplary embodiments.

[0055] In the relevant drawings

[0056] Figure 1 An embodiment of an optical layer system according to the invention as an optical interference filter with 4 different filter examples (ad) is shown;

[0057] Figure 2 Shown according to Figure 1 An exemplary transmission region of an interference filter according to the present invention;

[0058] Figure 3 shows a schematic diagram of a sputtering process for producing an optical layer system according to the invention;

[0059] Figure 4 An application example of the optical layer system according to the present invention as a TOF sensor for facial recognition is shown. DETAILED DESCRIPTION

[0060] Figure 1 An embodiment of an optical layer system according to the invention as an optical interference filter is shown. The optical interference filter is deposited on a substrate 1. For example, the deposition can be carried out using a sputtering process, a CVD process or an evaporation process (electron beam). The interference filter usually consists of a plurality of layers with different refractive indices and extinction coefficients. The plurality of layers form a layer stack, in which cavities and mirror systems are arranged alternately. The mirror system is in turn constructed or stacked from different mirror layers, in which high, low and / or medium refractive layers usually alternate. The optical thickness of the cavity corresponds to λ / 4 and the optical thickness of the mirror layer corresponds to λ / 2.

[0061] Figure 1 a) shows an example of a filter with two cavities 3 and a mirror system 2 made of a-Si:H. The two cavities 3 have the same refractive index ni, for example n 1 =3.1 and the mirror system 2 has two different refractive indices 21, 22, for example n 1 =3.1 and n 2 =3.6.

[0062] Figure 1 b) shows an example of a filter with two cavities 3 and a mirror system 2 made of a-Si:H. The two cavities 3 have different refractive indices n 1 31 and n 2 32, for example n 1 =3.1 and n 2 =3.6. The mirror layers 21, 22 of the mirror system also have different refractive indices, for example n1 =3.1 and n 2 =3.6.

[0063] Figure 1 c) shows an example of a filter with three cavities 3 and a mirror system 2 made of a-Si:H. The three cavities 3 have different refractive indices n 1 31.n 2 32 and n 3 33, for example n 1 =3.6, n 2 =3.2, n 3 =3.1. The mirror layers 21, 22 of the mirror system also have different refractive indices, for example n 1 =3.1 and n 3 =3.6.

[0064] Figure 1 d) shows an example of a filter with three cavities 3 and a mirror system 2 made of a-Si:H. The three cavities 3 have different refractive indices n 1 31.n 2 32 and n 3 33, for example n 1 =3.6, n 2 =3.2, n 3 =3.1. The mirror layers 21, 22, 23 of the mirror system also have different refractive indices, for example n 1 =3.6, n 2 =3.2, n 3 =3.1.

[0065] Figure 2 Shows Figure 1 0004] An exemplary transmission range of an interference filter according to the present invention is shown in Figure 1. By using only a-Si:H, the effective refractive index of the filter is higher than when a low refractive index material (e.g., silicon dioxide) is used. The transmission band shift is inversely proportional to the effective refractive index. In other words, the larger the effective refractive index, the smaller the shift of the transmission band.

[0066] Figure 3 A schematic diagram of a sputtering process for producing an optical layer system according to the invention is shown.

[0067] During sputtering deposition, energetic particles are directed onto the silicon target 7, wherein these particles have sufficient energy to sputter silicon atoms out of the target 7 and transfer them to the surface of the substrate 1 under the influence of a magnetic or electric field, thereby coating them. The sputtering gas may be, for example, argon (Ar) from an argon source. Alternatively, other ionizable inert gases, such as xenon, may also be used as sputtering gases.

[0068] Another production variant involves adjusting the reactive gas content 6 in a non-reactive or only partially reactive sputtered layer using a plasma and / or ion source 10. After deposition of a subnanometer thick layer, the sputtered layer is treated with the aid of a plasma and / or ion source 10 in order to set the desired stoichiometry.

[0069] To produce hydrogenated amorphous silicon, hydrogen enters the process chamber through a gas inlet during sputtering deposition. The amount of sputtering gas and hydrogen or other doping gas (if necessary) can be adjusted using a dynamic flow controller. This allows the required stoichiometry of the doping gas used to produce low, medium and high refractive index layers to be set and adjusted to ensure that the same optical properties are formed during the gas flow changes between the low, medium and high refractive index layers. The structure of hydrogen incorporation in silicon can also be influenced and controlled by process parameters such as substrate temperature, target bias (-V), process chamber pressure, total flow rate, etc.

[0070] The layer materials produced in this way are deposited on a substrate in a sequence and layer thicknesses predetermined with the aid of an optical model in order to meet optical requirements, for example, of an optical filter. Exact knowledge of the dependencies between the optical properties (refractive index and extinction coefficient) of the individual layers and the process parameters is an important prerequisite for being able to use the previously used models to make correct predictions about the properties of the optical layer system to be manufactured, for example, an optical filter, for simulation. For each high, low or medium refractive index layer, the process parameters (process pressure, gas flow, gas ratio, power of the sputtering source / plasma and / or ion source, temperature) are set precisely in order to be able to achieve reproducible layer properties.

[0071] The method according to the invention eliminates the need to switch between inlets for different sputtering materials, such as niobium pentoxide or silicon dioxide, or various doping gases, such as oxygen or hydrogen, for layers with different refractive indices. This also eliminates the need for long flushing times in the process chamber, which can increase productivity and improve layer properties. This is particularly important when a large number of end products are required.

[0072] Figure 4An example of the application of an optical layer system according to the invention as a TOF sensor for facial recognition is shown. The TOF sensor consists of a light source 11, typically a laser. It emits light 15, which is reflected by a three-dimensional object 14. The reflected light 16 is detected by a photodetector 12. It is advantageous if an optical filter 13 in the form of a bandpass filter is arranged in front of the photodetector 12. This filter ensures that only radiation with one wavelength emitted by the light source is detected and processed. For optimal functioning of the filter 13, it must have a high transmittance within the passband range and a very low transmittance outside the passband range. Furthermore, it is important that the filter has a large tolerance for wavelength shifts at different light incidence angles. These requirements must be taken into account in the design of the filter.

[0073] Reference numerals list

[0074] 1 substrate

[0075] 2 Mirror Layer

[0076] 21 Refractive index is n 1 The first mirror layer

[0077] 22 The refractive index is n 2 The second mirror layer

[0078] 23 Refractive index is n 3 The third mirror layer

[0079] 3 Cavity

[0080] 31 Refractive index is n 1 The first cavity

[0081] 32 Refractive index is n 2 The second cavity

[0082] 33 refractive index n 3 The third cavity

[0083] 4 Sputtering gas

[0084] 5 Sputtering particles

[0085] 6 Reactive Gases

[0086] 7 Sputtering Target

[0087] 8 substrate

[0088] 9 Coating

[0089] 10 Plasma source and / or ion source

[0090] 11 Light Source

[0091] 12 Photodetector

[0092] 13 Optical Filters

[0093] 14 Three-dimensional objects

[0094] 15 Light from the source

[0095] 16 Reflected light from a light source

Claims

1. A method for producing an optical layer system consisting of a plurality of layers, wherein the layers of the optical layer system are deposited onto a substrate from the same material by means of a selected coating method, wherein the material is hydrogenated amorphous silicon a-Si:H or hydrogenated germanium Ge:H, wherein the refractive index and extinction coefficient of each of the plurality of layers of the layer system are adjusted by controlling the process parameters of the selected coating method.

2. The method for producing an optical layer system according to claim 1, wherein: The same material is a-Si:H:x or Ge:H:x, where x contains nitrogen (N2) or chlorine (Cl2).

3. The method for producing an optical layer system according to claim 1, wherein: The coating method is a sputtering process, wherein the sputtering process is carried out by reacting with a reactive gas mixture of argon Ar and / or krypton Kr and / or helium He and / or xenon Xe and hydrogen H and / or nitrogen and / or chlorine, or sputtering is carried out using Ar, Kr, He and / or Xe, and the layers of the layer system are hydrogenated to form a-Si:H or Ge:H by means of a plasma and / or ion source, or the sputtering process is carried out as a combination of reactive sputtering and the plasma and / or ion source used, wherein the refractive index and extinction coefficient of each individual a-Si:H or Ge:H layer of the layer system is adjusted by the ratio of Ar, Kr, He and / or Xe to hydrogen.

4. The method for producing an optical layer system according to claim 1, wherein: The reactive gas mixture is argon Ar and nitrogen N, or argon Ar and oxygen O2.

5. The method for producing an optical layer system according to claim 1, wherein: The coating method is a chemical vapor deposition process, CVD process, wherein the CVD process is carried out with plasma assistance, by catalysis or by thermal treatment of an evaporator unit and a plasma source, wherein the refractive index and the extinction coefficient of each a-Si:H:x or Ge:H:x layer of the layer system are controlled by gas flow via the ratio of silane or germane to hydrogen and / or power regulation of the evaporator unit and the plasma source.

6. The method for producing an optical layer system according to claim 1, wherein: The coating method is an electron beam evaporation process in combination with an ion source, wherein the refractive index and the extinction coefficient of each a-Si:H:x or Ge:H:x layer of the layer system are adjusted by setting the absolute gas flow and / or the ratio of the partial gas flows in the gas mixture of the ion source and the power of the evaporator unit and the ion source.

7. The method for producing an optical layer system according to any one of claims 2 to 6, wherein: The optimum process parameters for setting a defined refractive index and extinction coefficient for each a-Si:H or Ge:H layer of the layer system are determined experimentally by preliminary tests or simulations.

8. An optical layer system manufactured according to the method of any one of claims 1 to 7, comprising a plurality of layers arranged on a substrate, wherein a portion of the layers has a high refractive index n H , and another part of the layer has a low refractive index n L , and another part of the layer has a medium refractive index n M , where n H >n M ≥n L , wherein layers with different refractive indices are alternately stacked and arranged, characterized in that The multiple layers are formed of the same material, wherein the high refractive index layer, the medium refractive index layer and the low refractive index layer differ only in the stoichiometry of their doping gases, and wherein the optical properties of the high refractive index layer, the medium refractive index layer and the low refractive index layer can be adjusted by adjusting the stoichiometry of the doping gas by a process control device.

9. The optical layer system according to claim 8, characterized in that The layer system has an average refractive index n My two or more layers of, where y is an integer greater than zero and n H >n M1 ≥n M2 ≥...≥n My >n L .

10. The optical layer system according to claim 8 or 9, characterized in that The same material is hydrogenated amorphous silicon a-Si:H or hydrogenated germanium Ge:H, and the doping gas is hydrogen H.

11. The optical layer system according to any one of claims 8 to 10, characterized in that The optical layer system is designed as a bandpass filter.

12. The optical layer system according to claim 11, characterized in that The bandpass filter consists of a layer sequence of high-refractive-index layers, medium-refractive-index layers and / or low-refractive-index layers, wherein for the wavelength range from 800 nm to 1100 nm: the refractive index n of the high-refractive-index layer made of a-Si:H is H =3.35 to 3.8, extinction coefficient k<0.001, refractive index n of medium refractive index layer M =3.0 to 3.6, k<0.001, the refractive index of the low refractive index layer n L =2.5 to 3.3, k<0.

001.

13. The optical layer system according to claim 10, characterized in that The bandpass filter is composed of a layer sequence of high- and low-refractive-index layers, medium- and low-refractive-index layers and / or low-refractive-index layers, wherein for the wavelength range from 900 nm to 980 nm: the refractive index n of the high-refractive-index layer made of a-Si:H is H =3.6 to 3.8, extinction coefficient k<0.0001, refractive index of medium refractive index layer n M =3.2 to 3.3, k<0.0001, the refractive index of the low refractive index layer n L =3.0 to 3.1, k<0.0001.

14. The optical layer system according to any one of claims 8 to 10, characterized in that The optical layer system is designed as a comb filter, wherein a refractive index gradient can be formed on the plurality of layers, and the refractive index gradient can be adjusted for each of the plurality of layers of the optical layer system by adjusting the stoichiometry of the doping gas by a process control device.

15. The optical layer system according to any one of claims 8 to 10, characterized in that The optical layer system is designed as an optical interference filter.