Surface coating material for electrical contact, and electrical contact, switch, and connector terminal using same
By optimizing the orientation and structure of the silver layer in the surface coating material of the electrical contact, combined with the intermediate layer, the wear problem of the electrical contact during the switching operation is solved, the bending processability and wear resistance are improved, the contact resistance is reduced, and a better Stable electrical connection.
Patent Information
- Application Number
- CN202380024470.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-30
- Filing Date
- 2023-05-16
- Publication Date
- 2024-10-15
AI Technical Summary
The surface coating materials of existing electrical contacts are easily worn during switching operations, resulting in increased contact resistance, and have poor bending processability, making it difficult to maintain durability in actual use environments.
By adjusting the peak intensity ratio obtained from the X-ray diffraction pattern of the silver-containing layer, the orientation and structure of the silver layer are optimized, and combined with the intermediate layer, the bending processability and wear resistance of the electrical contact are improved.
Significantly improves the bending processability and wear resistance of electrical contacts, reduces contact resistance, and ensures stable performance in actual use environments.
Smart Images

Figure CN118786252A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a surface covering material for an electric contact, and an electric contact, a switch and a connector terminal using the surface covering material for an electric contact. Background Art
[0002] In recent years, the electronic control of consumer electronic equipment and vehicle-mounted connection parts has been developing rapidly, and is gradually moving from the previous direct-cut contacts that directly cut off the power current to the addition of signal-cut contacts that cut off electrical signals. For the contacts of switches and connectors installed in these consumer electronic equipment and vehicle-mounted connection parts, the durability of sliding caused by repeated switching operations and sliding of connectors is sought, and these durability are evaluated by keying tests. In the keying test, in order to reduce the resistance of the contacts, surface coating materials for electrical contacts are used for these contacts, which are formed by applying a base plating composed of nickel (Ni) or the like on the surface of a conductive substrate containing copper (Cu), iron (Fe), and aluminum (Al) as the main components, and then further plating silver (Ag) and silver alloy thereon.
[0003] For example, Patent Document 1 describes a copper alloy composite foil, which is formed by providing a silver smooth layer on at least one surface of a copper alloy plate, and in the copper alloy composite foil, when the total of the intensity of the (220) crystal plane orientation and the intensity of the (111) crystal plane orientation obtained by X-ray diffraction method is set to 100, the intensity of the (200) crystal plane orientation on the surface of the silver smooth layer is in the range of greater than 34 and less than 100, and when the intensity of the (111) crystal plane orientation is set to 100, the intensity of the (220) crystal plane orientation is in the range of greater than 18 and less than 120.
[0004] [Prior Technical Literature]
[0005] (Patent Document)
[0006] Patent document 1: Japanese Patent Application Publication No. 2020-26566. Summary of the invention
[0007] [Problems that the invention aims to solve]
[0008] However, silver has the property of being easily worn due to adhesion, so the silver (Ag) and silver alloy plating applied to the surface is easily worn due to the sliding caused by the switching operation of the switch and the sliding of the connector, and thus has the disadvantage of increasing the contact resistance. In this regard, the copper alloy composite foil described in Patent Document 1 cannot suppress the adhesion of silver even if the peak intensity of the silver smooth layer obtained from the Ag (220) plane obtained from the X-ray diffraction pattern is increased to improve the hardness, so it still cannot improve the durability evaluated by the keying test. In addition, the copper alloy composite foil described in Patent Document 1 only focuses on the relationship between the peak intensities obtained from the Ag (200) plane, the Ag (220) plane and the Ag (111) plane obtained from the X-ray diffraction pattern of the silver smooth layer, and does not focus on the influence of other peak intensities.
[0009] Furthermore, although the copper alloy composite foil described in Patent Document 1 has been subjected to a sliding wear test using a steel ball as the target material, in an actual use environment, a problem may arise due to the wear caused by sliding with silver, which is more likely to adhere than a steel ball. Therefore, it is still desired to improve the wear resistance, which is evaluated by a typing test corresponding to the actual use environment.
[0010] Furthermore, the copper alloy composite foil described in Patent Document 1 is inferior in bending workability and its shape is not stable when formed into the shape of a terminal or a connector.
[0011] The object of the present invention is to provide a surface covering material for an electric contact and an electric contact, a switch and a connector terminal using the surface covering material for an electric contact, wherein the surface covering material for an electric contact has excellent bending workability and also has a silver-containing layer on the surface, and the silver-containing layer can suppress adhesion and improve wear resistance under conditions corresponding to actual use environments.
[0012] [Technical means to solve the problem]
[0013] The inventors studied all the peak intensities obtained from the X-ray diffraction pattern of the silver-containing layer and found that when the first total peak intensity is set to h1 and the second total peak intensity is set to h2, the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is set to a range of greater than 1.0 and less than 3.0, thereby improving the bending workability of the surface coating material for electrical contacts and improving the wear resistance of the silver-containing layer under conditions corresponding to the actual use environment, thereby completing the present invention, wherein the first total peak intensity is the total value of the peak intensity originating from the Ag (111) plane and the peak intensity originating from the plane parallel to the Ag (111) plane, and the second total peak intensity is the total value of the peak intensities remaining after subtracting the first total peak intensity (h1) from the total value of all detected peak intensities.
[0014] That is, the main configuration of the present invention is as follows.
[0015] (1) A surface coating material for an electric contact, comprising a conductive substrate and a silver-containing layer, wherein the silver-containing layer covers at least one side of the conductive substrate, wherein the surface coating material for an electric contact is characterized in that:
[0016] When the first total peak intensity obtained from the X-ray diffraction pattern of the silver-containing layer is set to h1 and the second total peak intensity is set to h2, the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is in the range of greater than 1.0 and less than 3.0, the first total peak intensity is the total value of the peak intensity originating from the Ag (111) plane and the peak intensity originating from the plane parallel to the Ag (111) plane, and the second total peak intensity is the total value of the peak intensities remaining after subtracting the first total peak intensity (h1) from the total value of all detected peak intensities.
[0017] (2) The surface covering material for an electric contact as described in (1) above, wherein the half width of a peak derived from the Ag (111) plane in the silver-containing layer is in the range of 0.15° to 0.30°.
[0018] (3) The surface covering material for an electric contact according to (1) or (2) above, wherein the silver-containing layer contains 99 mass % or more of silver.
[0019] (4) The surface covering material for an electric contact as described in any one of (1) to (3) above, wherein the conductive substrate is composed of pure copper, a copper alloy, pure iron, an iron alloy, pure aluminum or an aluminum alloy.
[0020] (5) The surface covering material for an electric contact as described in any one of (1) to (4) above, further comprising at least one intermediate layer between the conductive substrate and the silver-containing layer, wherein the intermediate layer is composed of pure copper, a copper alloy, pure nickel or a nickel alloy.
[0021] (6) The surface covering material for an electric contact according to any one of (1) to (5) above, wherein the conductive substrate has a thickness in a range of 0.03 mm to 0.30 mm.
[0022] (7) An electric contact produced by using the surface covering material for an electric contact according to any one of (1) to (6) above.
[0023] (8) A switch having the electric contact described in (7) above.
[0024] (9) A connector terminal having the electric contact described in (7) above.
[0025] [Effects of the Invention]
[0026] According to the present invention, there can be provided a surface covering material for an electric contact and an electric contact, a switch and a connector terminal using the surface covering material for an electric contact. The surface covering material for an electric contact has excellent bending workability and also has a silver-containing layer on the surface. The silver-containing layer can suppress adhesion and improve wear resistance under conditions corresponding to an actual use environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] FIG. 1 is a schematic diagram showing a cross section including the thickness direction of an example of the surface covering material for an electric contact of the present invention.
[0028] FIG. 2 is a schematic diagram showing a cross section including the thickness direction of a modified example of the surface covering material for an electric contact of the present invention having an intermediate layer. DETAILED DESCRIPTION
[0029] Below, while referring to the attached Figure 1 The specific embodiments of the present invention will be described in detail. The present invention is not limited to the following embodiments, and various modifications can be made within the scope of the gist of the present invention.
[0030] 1. Surface coating materials for electrical contacts
[0031] The surface coating material 1 for an electric contact of the present invention comprises a conductive substrate 2 and a silver-containing layer 3 coating at least one surface of the conductive substrate 2, wherein the silver-containing layer 3 has a ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) in a range of greater than 1.0 and less than 3.0 when a first total peak intensity obtained from an X-ray diffraction pattern is set as h1 and a second total peak intensity is set as h2, wherein the first total peak intensity is a total value of a peak intensity originating from a Ag (111) plane and a peak intensity originating from a plane parallel to the Ag (111) plane, and the second total peak intensity is a total value of peak intensities remaining after subtracting the first total peak intensity (h1) from the total value of all detected peak intensities.
[0032] As a result, the orientation of the silver contained in the silver-containing layer 3 is appropriately increased in the orientation that is excellent in keying property, that is, the ratio of the orientation that is not parallel to the Ag (111) plane relative to the total orientation. Therefore, even when silver that is easy to adhere is used as the target material corresponding to the actual use environment, the adhesion of silver in the keying test can be suppressed, and the wear of the silver-containing layer 3 due to adhesion can be suppressed. In addition, in the silver-containing layer 3, the ratio of the orientation that is parallel to the Ag (111) plane is relatively reduced, and the silver arranged in the orientation other than the orientation is relatively increased, thereby improving the bending workability of the surface coating material 1 for electric contacts. As a result, it is possible to provide a surface coating material 1 for electric contacts that is excellent in bending workability and further includes a silver-containing layer 3 on the surface, wherein the silver-containing layer 3 can suppress adhesion and improve wear resistance under conditions corresponding to the actual use environment.
[0033] (1) Surface Covering Material for Electric Contact According to One Embodiment
[0034] FIG. 1 is a schematic diagram showing a cross section including the thickness direction of an example of a surface coating material for an electric contact of the present invention. The surface coating material for an electric contact 1 comprises a conductive substrate 2 and a silver-containing layer 3 coating at least one side of the conductive substrate 2. In addition, in the surface coating material for an electric contact 1 of FIG. 1, the silver-containing layer 3 coats one side of the conductive substrate 2, but is not limited to this aspect, and the silver-containing layer 3 may also coat both sides of the conductive substrate 2.
[0035] Hereinafter, each part of the surface covering material 1 for an electric contact will be described in detail.
[0036] (Conductive substrate)
[0037] The conductive substrate 2 is made of pure copper, copper alloy, pure iron, iron alloy, pure aluminum or aluminum alloy.
[0038] Among them, copper alloys include Cu-Sn-P, Cu-Zn, Cu-Ni-Si, Cu-Sn-Ni, Cu-Cr-Mg, Cu-Ni-Si-Zn-Sn-Mg, etc. In addition, iron alloys include Fe-Cr-Ni, Fe-Cr, etc. In addition, aluminum alloys include Al-Mg, Al-Mg-Si, etc.
[0039] The shape of the conductive substrate 2 is not particularly limited and can be appropriately selected according to the application, but is preferably a strip-shaped material or a plate-shaped material, and can also be a rod-shaped material or a wire-shaped material. In addition, the conductive substrate 2 is preferably produced by rolling.
[0040] The conductivity of the conductive substrate 2 is not particularly limited, but is preferably 20% IACS or more, and more preferably 25% IACS or more. This allows the entire surface coating material 1 for electrical contacts to have excellent conductivity. Here, the conductivity (IACS; International Annealed Copper Standard) can be determined by measuring in a thermostatic chamber maintained at 20°C (±1°C) using a four-terminal method.
[0041] The conductive substrate 2 preferably has a thickness in the range of 0.03 mm or more and 0.30 mm or less. Here, by setting the thickness of the conductive substrate 2 to 0.30 mm or less, the surface covering material 1 for electric contacts having the conductive substrate 2 can be easily used as a contact material of a switch. On the other hand, by setting the thickness of the conductive substrate 2 to 0.03 mm or more, the mechanical strength of the conductive substrate 2 can be improved. In addition, the method for measuring the thickness of the conductive substrate 2 will be described later.
[0042] (Silver-containing layer)
[0043] The silver-containing layer 3 is provided in a manner of coating at least one side of the conductive substrate 2, and contains (Ag). Here, the silver-containing layer 3 is preferably composed of pure silver or a silver alloy containing more than 95% by mass of silver, and more preferably composed of pure silver containing more than 99% by mass of silver. Among these, the silver-containing layer 3 is particularly preferably composed of pure silver composed of silver and unavoidable impurities. By containing a large amount of silver in the silver-containing layer 3, the contact resistance value of the surface formed by the silver-containing layer 3 can be reduced, so that when the surface coating material 1 for electric contacts is used as an electric contact of a switch, a connector, etc., the electrical connectivity can be improved.
[0044] On the other hand, the silver-containing layer 3 may contain a second element, which is composed of one or more elements selected from the group consisting of zinc (Zn), copper (Cu), nickel (Ni), selenium (Se), antimony (Sb) and cobalt (Co). By including such a second element in the silver-containing layer 3, the typing property and wear resistance of the surface coating material 1 for electric contacts can be further improved. On the other hand, from the viewpoint of improving the electrical connectivity of the surface coating material 1 for electric contacts, the silver-containing layer 3 preferably contains one or more elements selected from the group consisting of zinc (Zn), copper (Cu), nickel (Ni), selenium (Se), antimony (Sb) and cobalt (Co) in a total amount of 5 mass % or less.
[0045] When the first total peak intensity obtained from the X-ray diffraction pattern of the silver-containing layer 3 is set to h1 and the second total peak intensity is set to h2, the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is in the range of greater than 1.0 and less than 3.0, the first total peak intensity is the total value of the peak intensity originating from the Ag (111) plane and the peak intensity originating from the plane parallel to the Ag (111) plane, and the second total peak intensity is the total value of the peak intensities remaining after subtracting the first total peak intensity (h1) from the total value of all detected peak intensities. In the surface coating material 1 for electric contact of the present invention, the orientation of silver contained in the silver-containing layer 3 is important. The crystal plane orientation of the Ag (111) plane and the plane parallel to the Ag (111) plane exposed on the surface of the silver-containing layer 3 has the property of reducing the keying property of the surface coating material 1 for electric contact. On the other hand, the crystal plane orientation of the plane not parallel to the Ag (111) plane exposed on the surface of the silver-containing layer 3 has the property of improving the keying property of the surface coating material 1 for electric contact. Therefore, in particular, by setting the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) in the range of 1.0 or more and 3.0 or less, the ratio of the peak intensity originating from the plane not parallel to the Ag (111) plane can be appropriately increased. As a result, even when pure silver is used as the target material, the adhesion of the silver-containing layer 3 can be suppressed to improve the wear resistance, and in particular, the keying property of the surface coating material 1 for electric contact can be improved.
[0046] Here, by setting the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) to 1.0 or more, it is possible to suppress the reduction in the bending workability of the surface coating material 1 for electric contacts caused by the excessive deformation of the crystals contained in the silver-containing layer 3, and in particular, it is possible to suppress the cracking of the silver-containing layer 3 during bending. In addition, by setting the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) to 3.0 or less, it is possible to relatively increase the ratio of the peak intensity originating from the surface that is not parallel to the Ag (111) surface, thereby suppressing the adhesion of the silver-containing layer 3 and improving the wear resistance.
[0047] As planes parallel to the Ag(111) plane, for example, the Ag(222) plane and the Ag(333) plane can be listed, but the peak intensity other than the Ag(222) plane shown in the X-ray diffraction pattern is relatively weak, so only the Ag(222) plane can be set as a plane parallel to the Ag(111) plane.
[0048] The half width of the peak derived from the Ag (111) plane of the silver-containing layer 3 obtained from the X-ray diffraction pattern is preferably in the range of 0.15° or more and 0.30° or less. In particular, by setting the half width of the peak derived from the Ag (111) plane to 0.30° or less, it is possible to suppress the reduction in the bending workability of the surface coating material 1 for electric contacts caused by the excessive deformation of the crystals contained in the silver-containing layer 3. In addition, by setting the half width of the peak derived from the Ag (111) plane to 0.15° or more, the deformation remaining in the crystals contained in the silver-containing layer 3 can be maintained high and the hardness of the silver-containing layer 3 will be increased, so that the typing property and wear resistance of the silver-containing layer 3 can be improved.
[0049] The thickness of the silver-containing layer 3 is not particularly limited, for example, it is preferably in the range of 0.05 μm or more and 10 μm or less. In particular, by setting the thickness of the silver-containing layer 3 to be 0.05 μm or more, the excellent typing property of the surface coating material 1 for electric contacts can be maintained over a longer period of time. Therefore, the thickness of the silver-containing layer 3 is preferably 0.05 μm or more, more preferably 0.10 μm or more, and further preferably 0.15 μm or more. On the other hand, by setting the thickness of the silver-containing layer 3 to be 10 μm or less, the cost of the surface coating material 1 for electric contacts can be suppressed. Therefore, the thickness of the silver-containing layer 3 is preferably 10 μm or less, more preferably 2.0 μm or less, and further preferably 1.0 μm or less. In addition, the method for measuring the thickness of the silver-containing layer 3 will be described later.
[0050] (2) Surface covering material for electric contact according to other embodiments
[0051] FIG. 2 is a schematic diagram showing a variation of the surface coating material for electric contacts of the present invention having an intermediate layer in a cross section including the thickness direction. The surface coating material for electric contacts 1A shown in FIG. 2 further has at least one intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3, and the intermediate layer 4 is composed of pure copper, copper alloy, pure nickel or nickel alloy. That is, the silver-containing layer 3 of the surface coating material for electric contacts 1A covers at least one side of the conductive substrate 2 through the intermediate layer 4. By having the surface coating material for electric contacts 1A having the intermediate layer 4, it is possible to suppress the heat diffusion of the elements constituting the conductive substrate 2 to the silver-containing layer 3, and to improve the adhesion between the conductive substrate 2 and the silver-containing layer 3.
[0052] Among them, examples of nickel alloys include Ni—P-based alloys, and examples of copper alloys include Cu—Sn-based alloys and Cu—Co-based alloys.
[0053] The thickness of the intermediate layer 4 is not particularly limited, and is preferably in the range of 0.01 μm or more and 1.00 μm or less. In particular, by setting the thickness of the intermediate layer 4 to be 0.01 μm or more, it is easy to suppress the thermal diffusion of the elements constituting the conductive substrate 2 to the silver-containing layer 3, and the adhesion between the conductive substrate 2 and the silver-containing layer 3 can be easily improved. On the other hand, by setting the thickness of the intermediate layer 4 to be 1.00 μm or less, the bending processability of the surface coating material 1A for electric contacts can be improved, and in particular, when the ratio of the bending radius to the thickness (R / t) is set to 1 to perform bending, the surface coating material 1A for electric contacts can be made less likely to be damaged.
[0054] The surface coating materials 1 and 1A for electric contacts constructed as described above have the property that abrasion caused by adhesion of the silver-containing layer 3 is not likely to occur, so it is preferred to use the surface coating materials 1 and 1A for electric contacts to make electric contacts, and in particular, it is preferred to construct the surface coating materials 1 and 1A in such a way that the silver-containing layer 3 is in electrical contact with the target material. At this time, even if the target material is silver that is easy to adhere, it is not easy to cause abrasion due to sliding caused by repeated switching operations of the switch and sliding of the connector terminal, so it can become difficult for the contact resistance of the electric contact to become high. In addition, the surface coating materials 1 and 1A for electric contacts are excellent in bending processability, so when formed into the shape of the terminal and the connector, the shape can be easily stabilized. Therefore, the surface coating materials 1 and 1A for electric contacts of the present invention can be applied to switches and connector terminals having electric contacts. Furthermore, such switches and connector terminals can be used in various electronic devices for civilian use and vehicle-mounted connection parts.
[0055] In the surface covering materials 1 and 1A for electric contacts of the present invention, the silver-containing layer 3 and the intermediate layer 4 covering the conductive substrate 2 may be formed on at least one surface of the conductive substrate 2 or on both surfaces of the conductive substrate 2 .
[0056] 3. Method for manufacturing surface coating material for electric contact
[0057] As an example of a method for producing the surface coating material 1 for electric contacts, there can be cited a method in which, after forming the silver-containing layer 3 on at least one side of the electrolytically degreased conductive substrate 2, the conductive substrate 2 having the silver-containing layer 3 formed on the surface is subjected to rolling processing. In particular, as a method for producing the surface coating material 1 for electric contacts having the intermediate layer 4, there can be cited a method in which, after sequentially forming the intermediate layer 4 and the silver-containing layer 3 on at least one side of the electrolytically degreased and acid-cleaned conductive substrate 2, the conductive substrate 2 having these layers formed on the surface is subjected to rolling processing.
[0058] As an example of the pretreatment of the conductive substrate 2, there can be cited a method of performing electrolytic degreasing and acid cleaning on the conductive substrate 2. Here, when the conductive substrate 2 is composed of pure iron or an iron alloy, as the pretreatment of the conductive substrate 2, after the electrolytic degreasing, the surface oxide film can be removed by acid electrolysis, and then nickel strike plating can be performed. In addition, when the conductive substrate 2 is composed of pure aluminum or an aluminum alloy, as the pretreatment of the conductive substrate 2, alkaline etching can be performed.
[0059] In addition, as a method for forming the silver-containing layer 3 and the intermediate layer 4, a plating method can be used, for example, wet plating such as electrolytic plating and electroless plating, and dry plating such as evaporation and sputtering can be used. Among these, from the viewpoint of efficiently forming a layer having a desired thickness, it is preferred to use a wet plating method, and it is more preferred to use electrolytic plating. For example, when the silver-containing layer 3 is formed, the electrolytic plating can be carried out under the following conditions: the bath temperature (liquid temperature) is an alkaline silver cyanide bath of 20°C or more and 25°C or less and 5A / dm 2 Above and 10A / dm 2 When the intermediate layer 4 is formed of pure copper or a copper alloy, electrolytic plating can be performed under the following conditions: a copper plating bath having a bath temperature (liquid temperature) of 40°C to 55°C and a current density of 5A / dm 2 Above and 10A / dm 2 When the intermediate layer 4 is formed of pure nickel or a nickel alloy, the electrolytic plating can be carried out under the following conditions: a nickel plating bath having a bath temperature (liquid temperature) of 45°C to 60°C and a current density of 5A / dm 2 Above and 15A / dm 2In particular, by adjusting the current density in the electrolytic plating when forming the silver-containing layer 3, the orientation of the silver contained in the silver-containing layer 3 can be controlled. In addition, the bath temperature and the current density value in the plating method can be adjusted in appropriate combination.
[0060] Then, the conductive substrate 2 having at least a silver-containing layer 3 formed on the surface is cold-rolled using a rolling work roll. By cold-rolling the conductive substrate 2 having a silver-containing layer 3 formed on the surface under appropriate conditions, the deformation amount of the crystal contained in the silver-containing layer 3 is appropriately increased, thereby adjusting the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) to a desired value. As a result, the typing property and wear resistance of the surface coating material 1 for electric contacts can be improved. At this time, cold rolling and heat treatment can be appropriately combined to implement.
[0061] The processing rate during cold rolling is preferably set in the range of more than 20% and less than 50%. In particular, by setting the processing rate during cold rolling to more than 20%, the deformation amount of the crystals contained in the silver-containing layer 3 will increase, for example, the half-width of the peak originating from the Ag (111) surface will become larger, thereby improving the typing property and wear resistance of the surface coating material 1 for electrical contacts. Therefore, the processing rate during cold rolling is preferably more than 20%, and more preferably more than 30%. On the other hand, if the processing rate during cold rolling is greater than 50%, the deformation amount of the crystals of the silver-containing layer 3 will become excessive, for example, the half-width of the peak originating from the Ag (111) surface will become larger than required, and the bending property of the surface coating material 1 for electrical contacts will be reduced. Therefore, the processing rate during cold rolling is preferably less than 50%, and more preferably less than 40%.
[0062] Here, the "processing ratio" (compression ratio) is a value expressed as a percentage by subtracting the cross-sectional area after rolling from the cross-sectional area before rolling, dividing by the cross-sectional area before rolling and then multiplying by 100, and can be expressed by the following formula.
[0063] [Processing rate] = {([Cross-sectional area before rolling] - [Cross-sectional area after rolling]) / [Cross-sectional area before rolling]} × 100 (%)
[0064] In addition, in the cold rolling, the diameter (roller diameter) of the rolling work roll in contact with the conductive substrate 2 on which the silver-containing layer 3 is formed can be set, for example, in the range of 70 mm or more and 90 mm or less from the viewpoint of setting the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) within a desired range. Here, if the diameter of the rolling work roll is small, there is a tendency that the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is adjusted to be larger.
[0065] After cold rolling or other rolling processing, the conductive substrate 2 having the silver-containing layer 3 formed thereon may be subjected to heat treatment. By combining rolling processing and heat treatment on the conductive substrate 2 having the silver-containing layer 3 formed thereon, the orientation of silver contained in the silver-containing layer 3 can be controlled.
[0066] The embodiments of the present invention are described above, but the present invention is not limited to the above embodiments, but includes all aspects within the concept of the present invention and the scope of the invention claims, and various changes can be made within the scope of the present invention.
[0067] [Example]
[0068] Next, in order to further clarify the effects of the present invention, examples of the present invention and comparative examples will be described, but the present invention is not limited to these examples of the present invention.
[0069] The surface covering materials for electric contacts of Examples 1 to 57 and Comparative Examples 1 to 54 were prepared by any of the following preparation methods A to I. The structures and properties of the prepared samples were evaluated and are shown in Tables 1 to 4 together with the preparation conditions.
[0070] (Measurement of Thickness of Silver-Containing Layer 3 and Intermediate Layer 4)
[0071] The obtained surface coating material 1, 1A for electric contact is cut on a surface parallel to the rolling direction of the conductive substrate 2 and along the thickness direction using an ion beam cross section polisher (Cross Section Polisher, manufactured by JEOL Ltd.), and then the thickness of the silver-containing layer 3 and the intermediate layer 4 exposed on the cut surface is measured using a scanning electron microscope (SEM).
[0072] (Measurement of Silver Content of Silver-Containing Layer 3)
[0073] The silver content (mass %) in the surface of the silver-containing layer 3 of the obtained surface covering material for electric contact 1 was measured using an electron probe microanalyzer (EPMA).
[0074] (Method for measuring the ratio of the first total peak intensity to the second total peak intensity)
[0075] The surface of the silver-containing layer 3 of the obtained surface coating material 1 for electric contacts was analyzed by X-ray diffraction method and analyzed by an X-ray diffraction device (manufactured by PANalytical Co., Ltd., model: X'Pert PRO). Then, based on the obtained X-ray diffraction pattern of the diffraction angle (2θ) and the diffraction peak intensity, the sum of the peak intensity originating from the Ag (111) plane and the peak intensity originating from the plane parallel to the Ag (111) plane was set as the first total peak intensity h1, and the total value of the peak intensities remaining after deducting the first total peak intensity h1 from the total value of all detected peak intensities was set as the second total peak intensity h2, and the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) at this time was calculated.
[0076] (Method for measuring half width of peak originating from Ag (111) surface)
[0077] The surface of the silver-containing layer 3 of the obtained surface coating material 1 for electric contacts was analyzed by X-ray diffraction method and analyzed by using an X-ray diffraction device (manufactured by PANalytical Co., Ltd., model: X'Pert PRO), and then the half-width of the peak originating from the Ag (111) plane was calculated based on the obtained X-ray diffraction pattern of the diffraction angle (2θ) and the diffraction peak intensity.
[0078] (Evaluation of the wear resistance of steel balls)
[0079] A steel ball as a target material was brought into contact with the surface of the obtained surface coating material for electric contact 1 on which the silver-containing layer 3 was formed, and then a friction and wear tester Tribo Gear (surface property measuring machine TYPE: 14FW, manufactured by Shinto Scientific Co., Ltd.) was used to perform 1000 reciprocating slides at the same location under the conditions of a contact load of 1N, a sliding distance of 50mm, and a sliding speed of 100mm / min. Then, a laser roughness meter was used to measure the depth from the reference surface (surface that has not been reciprocated) of the sliding portion of the target material to calculate the ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3. Based on the calculated ratio, the wear resistance of the steel ball was evaluated using the following criteria.
[0080] ⊚: The ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3 is less than 1 / 10.
[0081] ○: The ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3 is 1 / 10 or more and less than 1 / 5.
[0082] ×: The ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3 is 1 / 5 or more.
[0083] (Evaluation of the wear resistance of pure silver balls)
[0084] A pure silver ball as a target material was brought into contact with the surface of the obtained surface coating material for electric contact 1 on which the silver-containing layer 3 was formed, and then a friction and wear tester Tribo Gear (surface property measuring machine TYPE: 14FW, manufactured by Shinto Scientific Co., Ltd.) was used to perform 50 reciprocating slides at the same location under the conditions of a contact load of 4N, a sliding distance of 50mm, and a sliding speed of 100mm / min. Then, a laser roughness meter was used to measure the depth from the reference surface (surface that has not been reciprocated) of the sliding portion of the target material to calculate the ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3. Based on the calculated ratio, the wear resistance to the steel ball was evaluated using the following criteria.
[0085] ⊚: The ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3 is less than 1 / 10.
[0086] ○: The ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3 is 1 / 10 or more and less than 1 / 5.
[0087] ×: The ratio of the depth of the sliding portion to the thickness of the silver-containing layer 3 is 1 / 5 or more.
[0088] (Type test)
[0089] The obtained electric contact surface coating material 1 was processed into a fixed contact, and then a bell-shaped movable contact with a diameter of 4 mm composed of a silver-coated stainless steel bar was used as a movable contact on the surface formed with the silver-containing layer 3 to perform a keying test. The test conditions were a contact pressure of 9.8 N / mm 2 , typing speed 5Hz to perform 1 million times of typing, and then measure the contact resistance value before and after typing with a current value of 10mA, and use the following criteria to evaluate the change in contact resistance value before and after typing. In addition, if the contact is poor before the number of typing reaches 1 million times and the contact resistance cannot be measured, the typing and contact resistance measurement are terminated at this time point and evaluated as "×".
[0090] ◎: The change in contact resistance is less than 15 mΩ.
[0091] ○: The change in contact resistance value is 15 mΩ or more and less than 30 mΩ.
[0092] ×: The contact resistance cannot be measured when the change in contact resistance value is 30 mΩ or more or the number of keystrokes reaches 1 million times.
[0093] (Evaluation of bending workability)
[0094] The obtained surface covering material 1 for electric contact was subjected to a bending test based on the technical standard T307:2007 (Bending workability evaluation method of copper and copper alloy thin strip) of the Japan Copper Association, and the bending part was observed using an optical microscope. Then, the bending workability was evaluated based on the observation results obtained by referring to the technical standard T307:2007 of the Japan Copper Association. More specifically, the bending workability of the surface covering material 1 for electric contact was evaluated by taking five test pieces of 30 mm in length and 10 mm in width from the surface covering material 1 for electric contact so that the rolling direction became the length direction, and then bending was performed with the ratio of the bending radius to the thickness (R / t) being 1 and the bending angle being 90 degrees for each test piece, and then the surface covering material 1 for electric contact was evaluated for cracks and for lines formed on the surface of the surface covering material 1 for electric contact.
[0095] ◎: None of the five test pieces had cracks or cracks.
[0096] ○: Scratches occurred on the surface of one or more test pieces, but cracks did not occur on any of the five test pieces.
[0097] ×: The surface of one or more test pieces was cracked.
[0098] (Evaluation of contact resistance value)
[0099] For the surface of the obtained surface coating material 1 for electric contact having the silver-containing layer 3 formed thereon, the contact resistance values at any 10 locations were measured with a current value of 20 mA while applying a load of 1 N using an electric contact simulator (manufactured by Yamazaki Seiki Laboratories, Ltd.), and the average value (n=10) of the obtained measured values was set as the contact resistance value of the contact metal material, and then evaluated using the following criteria.
[0100] ◎: Contact resistance value is less than 0.5mΩ.
[0101] ○: The contact resistance value is 0.5 mΩ or more and less than 1.0 mΩ.
[0102] ×: The contact resistance value is 1.0 mΩ or more.
[0103] (Evaluation of heat resistance)
[0104] The obtained surface coating material 1 for electric contact was heated at 150°C for 1000 hours in an atmospheric atmosphere. After heating, the contact resistance values at 10 random locations on the surface of the surface coating material 1 for electric contact on which the silver-containing layer 3 was formed were measured using an electric contact simulator (manufactured by Yamazaki Seiki Laboratories, Ltd.) while applying a load of 1N and a current value of 20 mA, and the average value (n=10) of the obtained measured values was set as the contact resistance value of the metal material for the contact, and then the heat resistance was evaluated using the following criteria.
[0105] ◎: Contact resistance value is less than 1.0mΩ.
[0106] ○: The contact resistance value is 1.0 mΩ or more and less than 5.0 mΩ.
[0107] ×: The contact resistance value is 5.0 mΩ or more.
[0108] [Inventive Examples 1 to 11, 18, 19, Comparative Examples 13 to 18: Production Method A]
[0109] In Examples 1 to 7 of the present invention, C2680, which is a copper alloy (Cu-Zn system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Examples 8 to 11 of the present invention, C5212, which is a copper alloy (Cu-Sn-P system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Example 18 of the present invention, SUS301, which is an iron alloy (Fe-Cr-Ni system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Example 19 of the present invention, SUS304, which is an iron alloy (Fe-Cr-Ni system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Comparative Examples 13 to 18, C1100, which is pure copper and having a thickness as described in Table 2, was used as the conductive substrate 2.
[0110] As pretreatment of the conductive substrate 2, in Examples 1 to 11 of the present invention and Comparative Examples 13 to 18, electrolytic degreasing and acid cleaning were performed on the conductive substrate 2. In addition, as pretreatment of the conductive substrate 2 in Examples 18 and 19 of the present invention, after electrolytic degreasing, the oxide film on the surface was removed by acid electrolysis, and then nickel strike plating was performed by a nickel plating bath containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid.
[0111] Then, an aqueous solution containing 50 g / L of silver cyanide and 100 g / L of potassium cyanide was prepared as an electrolytic plating solution. Then, 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic cell with an inner diameter of 120 mm, and the conductive substrate 2 obtained after acid washing in the alkaline silver cyanide bath was immersed in the bath at a temperature of 25°C and a current of 10 A / dm2 The silver-containing layer 3 is formed on the surface of the conductive substrate 2 by electrolytic plating by passing electricity at a current density of , and then, using rolling work rolls having diameters shown in Tables 3 and 4, cold rolling is performed at the processing rates shown in Tables 3 and 4, thereby producing a surface covering material 1 for electric contacts, which has a silver-containing layer 3 covering the conductive substrate 2.
[0112] [Inventive Examples 12 to 14, Comparative Examples 1 to 6: Production Method B]
[0113] In Examples 12 to 14 of the present invention, pure copper, namely C1100, having a thickness as described in Table 1 was used as the conductive substrate 2. In Comparative Examples 1 to 6, copper alloy (Cu-Zn system), namely C2680, having a thickness as described in Table 2 was used as the conductive substrate 2. Each conductive substrate 2 was subjected to electrolytic degreasing and acid cleaning.
[0114] For Example 12 of the present invention and Comparative Examples 1 and 2, the electrolytic plating solution further contained zinc (Zn) as a second element, so an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 10 g / L of zinc chloride was modulated. In addition, for Example 13 of the present invention and Comparative Examples 3 and 4, the electrolytic plating solution further contained copper (Cu) as a second element, so an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 12 g / L of copper chloride dihydrate was modulated. In addition, for Example 14 of the present invention and Comparative Examples 5 and 6, the electrolytic plating solution further contained nickel (Ni) as a second element, so an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 12 g / L of nickel chloride was modulated.
[0115] 3 L of electrolytic plating solution was poured into a cylindrical plating electrolytic cell with an inner diameter of 120 mm, and the conductive substrate 2 obtained after acid washing in the alkaline silver cyanide bath was immersed in the bath at a temperature of 25° C. and a current of 10 A / dm 2 The silver-containing layer 3 is formed on the surface of the conductive substrate 2 by electrolytic plating by passing electricity at a current density of , and then, using rolling work rolls having diameters shown in Tables 3 and 4, cold rolling is performed at the processing rates shown in Tables 3 and 4, thereby producing a surface covering material 1 for electric contacts, which has a silver-containing layer 3 covering the conductive substrate 2.
[0116] [Inventive Examples 15 to 17, Comparative Examples 7 to 12: Production Method C]
[0117] In Examples 15 to 17 of the present invention, pure copper, namely C1100, having a thickness as described in Table 1 was used as the conductive substrate 2. In Comparative Examples 7 to 12, copper alloy (Cu-Zn system), namely C2680, having a thickness as described in Table 2 was used as the conductive substrate 2. Each conductive substrate 2 was subjected to electrolytic degreasing and acid cleaning.
[0118] For Example 15 of the present invention and Comparative Examples 7 and 8, the electrolytic plating solution further includes selenium (Se) as a second element, so an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 2.2 mg / L of potassium selenocyanate is modulated. In addition, for Example 16 of the present invention and Comparative Examples 9 and 10, the electrolytic plating solution further includes antimony (Sb) as a second element, so an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 12 g / L of antimony trichloride is modulated. In addition, for Example 17 of the present invention and Comparative Examples 11 and 12, the electrolytic plating solution further includes cobalt (Co) as a second element, so an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 10 g / L of cobalt chloride is modulated.
[0119] 3 L of electrolytic plating solution was poured into a cylindrical plating electrolytic cell with an inner diameter of 120 mm, and the conductive substrate 2 obtained after acid washing in the alkaline silver cyanide bath was immersed in the bath at a temperature of 25° C. and a current of 10 A / dm 2 The silver-containing layer 3 is formed on the surface of the conductive substrate 2 by electrolytic plating by passing electricity at a current density of , and then, using rolling work rolls having diameters shown in Tables 3 and 4, cold rolling is performed at the processing rates shown in Tables 3 and 4, thereby producing a surface covering material 1 for electric contacts, which has a silver-containing layer 3 covering the conductive substrate 2.
[0120] [Inventive Examples 20 to 30, 37, 38 Comparative Examples 31 to 36: Production Method D]
[0121] In Examples 20 to 26 of the present invention, C2680, which is a copper alloy (Cu-Zn system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Examples 27 to 30 of the present invention, C5212, which is a copper alloy (Cu-Sn-P system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Example 37 of the present invention, SUS301, which is an iron alloy (Fe-Cr-Ni system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Example 38 of the present invention, pure aluminum, which is A1050, having a thickness as described in Table 1, was used as the conductive substrate 2. In Comparative Examples 31 to 36, C1100, which is pure copper and having a thickness as described in Table 2, was used as the conductive substrate 2.
[0122] As pretreatment of the conductive substrate 2, electrolytic degreasing and acid cleaning were performed on the conductive substrate 2 in Examples 20 to 30 of the present invention and Comparative Examples 31 to 36. In addition, as pretreatment of the conductive substrate 2 in Example 37 of the present invention, after electrolytic degreasing, the oxide film on the surface was removed by acid electrolysis, and then nickel strike plating was performed by a nickel plating bath containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid. In addition, as pretreatment of the conductive substrate 2 in Example 38 of the present invention, alkaline etching was performed by an aqueous solution containing 100 g / L of sodium hydroxide and 10 g / L of sodium gluconate.
[0123] Then, an aqueous solution containing 23 g / L copper cyanide, 34 g / L sodium cyanide and 15 g / L sodium carbonate was prepared as an electrolytic plating solution for forming the intermediate layer 4. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate 2 obtained after acid washing in the copper plating bath was immersed in the bath temperature of 40°C at 5 A / dm 2 By passing electricity at a current density of , an intermediate layer 4 composed of pure copper is formed on the surface of the conductive base material 2 by electrolytic plating.
[0124] Next, an aqueous solution containing 50 g / L of silver cyanide and 100 g / L of potassium cyanide was prepared as an electrolytic plating solution for forming the silver-containing layer 3. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic cell with an inner diameter of 120 mm, and the obtained conductive substrate 2 having the intermediate layer 4 was immersed in an alkaline silver cyanide bath at a bath temperature of 25° C. and a current of 10 A / dm 2 The silver-containing layer 3 is formed on the surface of the intermediate layer 4 by electrolytic plating by passing electricity at a current density of , thereby forming the silver-containing layer 3 on the surface of the intermediate layer 4. Then, cold rolling is performed at the processing rates shown in Tables 3 and 4 using rolling work rolls having diameters shown in Tables 3 and 4, thereby producing a surface covering material 1A for electric contacts, which includes the silver-containing layer 3 covering the conductive substrate 2 and further includes the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3.
[0125] [Inventive Examples 31 to 33, Comparative Examples 19 to 24: Production Method E]
[0126] In Examples 31 to 33 of the present invention, pure copper, namely C1100, having a thickness as described in Table 1 was used as the conductive substrate 2. In Comparative Examples 19 to 24, copper alloy (Cu-Zn system), namely C2680, having a thickness as described in Table 2 was used as the conductive substrate 2.
[0127] After electrolytic degreasing and pickling of the conductive substrate 2, an aqueous solution containing 23 g / L copper cyanide, 34 g / L sodium cyanide and 15 g / L sodium carbonate was prepared as an electrolytic plating solution for forming the intermediate layer 4. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate 2 obtained after pickling in the copper plating bath was immersed in the bath temperature of 40°C at 5 A / dm 2 By passing electricity at a current density of , an intermediate layer 4 composed of pure copper is formed on the surface of the conductive base material 2 by electrolytic plating.
[0128] Next, for Example 31 of the present invention and Comparative Examples 19 and 20, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 10 g / L of zinc chloride was prepared as an electrolytic plating solution for forming the silver-containing layer 3 in order to make the silver-containing layer 3 contain zinc (Zn) as the second element. Furthermore, for Example 32 of the present invention and Comparative Examples 21 and 22, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of cupric chloride dihydrate was prepared as an electrolytic plating solution for forming the silver-containing layer 3 in order to make the silver-containing layer 3 contain copper (Cu) as the second element. In addition, for Example 33 of the present invention and Comparative Examples 23 and 24, as an electrolytic plating solution for forming the silver-containing layer 3, in order to make the silver-containing layer 3 contain nickel (Ni) as the second element, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 12 g / L of nickel chloride is prepared.
[0129] 3 L of electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the obtained conductive substrate 2 having the intermediate layer 4 was immersed in an alkaline silver cyanide bath at a bath temperature of 25° C. and a current of 10 A / dm 2 The silver-containing layer 3 is formed on the surface of the intermediate layer 4 by electrolytic plating by passing electricity at a current density of , thereby forming the silver-containing layer 3 on the surface of the intermediate layer 4. Then, cold rolling is performed at the processing rates shown in Tables 3 and 4 using rolling work rolls having diameters shown in Tables 3 and 4, thereby producing a surface covering material 1A for electric contacts, which includes the silver-containing layer 3 covering the conductive substrate 2 and further includes the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3.
[0130] [Inventive Examples 34 to 36, Comparative Examples 25 to 30: Production Method F]
[0131] In Examples 34 to 36 of the present invention, pure copper, namely C1100, having a thickness as described in Table 1 was used as the conductive substrate 2. In Comparative Examples 25 to 30, copper alloy (Cu-Zn system), namely C2680, having a thickness as described in Table 2 was used as the conductive substrate 2.
[0132] After electrolytic degreasing and pickling of the conductive substrate 2, an aqueous solution containing 23 g / L copper cyanide, 34 g / L sodium cyanide and 15 g / L sodium carbonate was prepared as an electrolytic plating solution for forming the intermediate layer 4. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate 2 obtained after pickling in the copper plating bath was immersed in the bath temperature of 40°C at 5 A / dm 2 By passing electricity at a current density of , an intermediate layer 4 composed of pure copper is formed on the surface of the conductive base material 2 by electrolytic plating.
[0133] Next, for Example 34 of the present invention and Comparative Examples 25 and 26, as the electrolytic plating solution for forming the silver-containing layer 3, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 2.2 mg / L of potassium selenocyanate was prepared in order to make the silver-containing layer 3 contain selenium (Se) as the second element. Furthermore, for Example 35 of the present invention and Comparative Examples 27 and 28, as the electrolytic plating solution for forming the silver-containing layer 3, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared in order to make the silver-containing layer 3 contain antimony (Sb) as the second element. In addition, for Example 36 of the present invention and Comparative Examples 29 and 30, as an electrolytic plating solution for forming the silver-containing layer 3, in order to make the silver-containing layer 3 contain cobalt (Co) as the second element, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 10 g / L of cobalt chloride was prepared.
[0134] 3 L of electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the obtained conductive substrate 2 having the intermediate layer 4 was immersed in an alkaline silver cyanide bath at a bath temperature of 25° C. and a current of 10 A / dm 2 The silver-containing layer 3 is formed on the surface of the intermediate layer 4 by electrolytic plating by passing electricity at a current density of , thereby forming the silver-containing layer 3 on the surface of the intermediate layer 4. Then, cold rolling is performed at the processing rates shown in Tables 3 and 4 using rolling work rolls having diameters shown in Tables 3 and 4, thereby producing a surface covering material 1A for electric contacts, which includes the silver-containing layer 3 covering the surface of the conductive substrate 2 and further includes the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3.
[0135] [Inventive Examples 39 to 49, 56, 57, Comparative Examples 49 to 54: Production Method G]
[0136] In Examples 39 to 45 of the present invention, C2680, which is a copper alloy (Cu-Zn system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Examples 46 to 49 of the present invention, C5212, which is a copper alloy (Cu-Sn-P system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Example 56 of the present invention, SUS301, which is an iron alloy (Fe-Cr-Ni system) having a thickness as described in Table 1, was used as the conductive substrate 2. In Example 57 of the present invention, pure aluminum, which is A1050, having a thickness as described in Table 1, was used as the conductive substrate 2. In Comparative Examples 49 to 54, C1100, which is pure copper and having a thickness as described in Table 2, was used as the conductive substrate 2.
[0137] As pretreatment of the conductive substrate 2, electrolytic degreasing and acid cleaning were performed on the conductive substrate 2 in Examples 39 to 49 of the present invention and Comparative Examples 49 to 54. In addition, as pretreatment of the conductive substrate 2 in Example 56 of the present invention, after electrolytic degreasing, the oxide film on the surface was removed by acid electrolysis, and then nickel strike plating was performed by a nickel plating bath containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid. In addition, as pretreatment of the conductive substrate 2 in Example 57 of the present invention, alkaline etching was performed by an aqueous solution containing 100 g / L of sodium hydroxide and 10 g / L of sodium gluconate.
[0138] Then, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride, and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming the intermediate layer 4. 3 L of the electrolytic plating solution was poured into a cylindrical electrolytic plating tank with an inner diameter of 120 mm, and the conductive substrate 2 obtained after acid washing in the copper plating bath was immersed in the bath at a bath temperature of 55°C and a current of 15 A / dm 2 By passing electricity at a current density of , an intermediate layer 4 composed of pure nickel is formed on the surface of the conductive base material 2 by electrolytic plating.
[0139] Next, an aqueous solution containing 50 g / L of silver cyanide and 100 g / L of potassium cyanide was prepared as an electrolytic plating solution for forming the silver-containing layer 3. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic cell with an inner diameter of 120 mm, and the obtained conductive substrate 2 having the intermediate layer 4 was immersed in an alkaline silver cyanide bath at a bath temperature of 25° C. and a current of 10 A / dm 2The silver-containing layer 3 is formed on the surface of the intermediate layer 4 by electrolytic plating by passing electricity at a current density of , thereby forming the silver-containing layer 3 on the surface of the intermediate layer 4. Then, cold rolling is performed at the processing rates shown in Tables 3 and 4 using rolling work rolls having diameters shown in Tables 3 and 4, thereby producing a surface covering material 1A for electric contacts, which includes the silver-containing layer 3 covering the conductive substrate 2 and further includes the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3.
[0140] [Inventive Examples 50 to 52, Comparative Examples 37 to 42: Production Method H]
[0141] In Examples 50 to 52 of the present invention, pure copper, namely C1100, having a thickness as described in Table 1 was used as the conductive substrate 2. In Comparative Examples 37 to 42, copper alloy (Cu-Zn system), namely C2680, having a thickness as described in Table 2 was used as the conductive substrate 2.
[0142] After electrolytic degreasing and pickling of the conductive substrate 2, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming the intermediate layer 4. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate 2 obtained after pickling in the copper plating bath was immersed in the bath temperature of 55°C at 15 A / dm 2 By passing electricity at a current density of , an intermediate layer 4 composed of pure nickel is formed on the surface of the conductive base material 2 by electrolytic plating.
[0143] Next, for Example 50 of the present invention and Comparative Examples 37 and 38, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 10 g / L of zinc chloride was prepared as an electrolytic plating solution for forming the silver-containing layer 3 in order to make the silver-containing layer 3 contain zinc (Zn) as the second element. Furthermore, for Example 51 of the present invention and Comparative Examples 39 and 40, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of cupric chloride dihydrate was prepared as an electrolytic plating solution for forming the silver-containing layer 3 in order to make the silver-containing layer 3 contain copper (Cu) as the second element. In addition, for Example 52 of the present invention and Comparative Examples 41 and 42, as an electrolytic plating solution for forming the silver-containing layer 3, in order to make the silver-containing layer 3 contain nickel (Ni) as the second element, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 12 g / L of nickel chloride was prepared.
[0144] 3 L of electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the obtained conductive substrate 2 having the intermediate layer 4 was immersed in an alkaline silver cyanide bath at a bath temperature of 25° C. and a current of 10 A / dm 2The silver-containing layer 3 is formed on the surface of the intermediate layer 4 by electrolytic plating by passing electricity at a current density of , thereby forming the silver-containing layer 3 on the surface of the intermediate layer 4. Then, cold rolling is performed at the processing rates shown in Tables 3 and 4 using rolling work rolls having diameters shown in Tables 3 and 4, thereby producing a surface covering material 1A for electric contacts, which includes the silver-containing layer 3 covering the conductive substrate 2 and further includes the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3.
[0145] [Inventive Examples 53 to 55, Comparative Examples 43 to 48: Production Method I]
[0146] In Examples 53 to 55 of the present invention, pure copper, namely C1100, having a thickness as described in Table 1 was used as the conductive substrate 2. In Comparative Examples 43 to 48, copper alloy (Cu-Zn system), namely C2680, having a thickness as described in Table 2 was used as the conductive substrate 2. Electrolytic degreasing and acid cleaning were performed on each conductive substrate 2.
[0147] After electrolytic degreasing and pickling of the conductive substrate 2, an aqueous solution containing 500 g / L of nickel sulfate hexahydrate, 30 g / L of nickel chloride and 30 g / L of sulfuric acid was prepared as an electrolytic plating solution for forming the intermediate layer 4. 3 L of the electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the conductive substrate 2 obtained after pickling in the copper plating bath was immersed in the bath temperature of 55°C at 15 A / dm 2 By passing electricity at a current density of , an intermediate layer 4 composed of pure nickel is formed on the surface of the conductive base material 2 by electrolytic plating.
[0148] Next, for Example 53 of the present invention and Comparative Examples 43 and 44, as an electrolytic plating solution for forming the silver-containing layer 3, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 2.2 mg / L of potassium selenocyanate was prepared in order to make the silver-containing layer 3 contain selenium (Se) as the second element. In addition, for Example 54 of the present invention and Comparative Examples 45 and 46, as an electrolytic plating solution for forming the silver-containing layer 3, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide, and 12 g / L of antimony trichloride was prepared in order to make the silver-containing layer 3 contain antimony (Sb) as the second element. In addition, for Example 55 of the present invention and Comparative Examples 47 and 48, as an electrolytic plating solution for forming the silver-containing layer 3, in order to make the silver-containing layer 3 contain cobalt (Co) as the second element, an aqueous solution containing 50 g / L of silver cyanide, 100 g / L of potassium cyanide and 10 g / L of cobalt chloride is prepared.
[0149] 3 L of electrolytic plating solution was poured into a cylindrical plating electrolytic tank with an inner diameter of 120 mm, and the obtained conductive substrate 2 having the intermediate layer 4 was immersed in an alkaline silver cyanide bath at a bath temperature of 25° C. and a current of 10 A / dm2 The silver-containing layer 3 is formed on the surface of the intermediate layer 4 by electrolytic plating by passing electricity at a current density of , thereby forming the silver-containing layer 3 on the surface of the intermediate layer 4. Then, cold rolling is performed at the processing rates shown in Tables 3 and 4 using rolling work rolls having diameters shown in Tables 3 and 4, thereby producing a surface covering material 1A for electric contacts, which includes the silver-containing layer 3 covering the conductive substrate 2 and further includes the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3.
[0150] [Table 1]
[0151]
[0152]
[0153] [Table 2]
[0154]
[0155]
[0156] (Notes) The underlined bold characters in the table indicate that they are outside the scope of the present invention.
[0157] [Table 3]
[0158]
[0159]
[0160] [Table 4]
[0161]
[0162]
[0163]
[0164] (Note) The numbers in bold with underline in the table indicate that the evaluation results were unacceptable.
[0165] As can be seen from Tables 1 to 4 above, the surface coating materials for electric contacts obtained from Examples 1 to 57 of the present invention, when the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is set to a range of 1.0 or more and 3.0 or less, the bending workability is evaluated as "◎" or "○", and the wear resistance of the silver-containing layer when silver is used as the target material is also evaluated as "◎" or "○". In addition, the surface coating materials for electric contacts of Examples 1 to 57 of the present invention are also evaluated as "◎" or "○" in the results of the keying test. In addition, the contact resistance of the silver-containing layer of the surface coating materials for electric contacts of Examples 1 to 57 of the present invention is low, and is evaluated as "◎" or "○", and the contact resistance of the silver-containing layer after heating is also low, and the heat resistance is also evaluated as "◎" or "○".
[0166] Therefore, the surface covering materials for electric contacts obtained in Examples 1 to 57 of the present invention are excellent in bending workability, and the silver-containing layer also has high wear resistance.
[0167] In contrast, in the surface covering materials for electric contacts obtained from Comparative Examples 1 to 54, the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) did not satisfy the range of greater than 1.0 and less than 3.0, and at least one of the bending workability and the wear resistance of the silver-containing layer when silver was used as the target material was evaluated as "×".
[0168] In particular, the surface covering material for electric contacts obtained by the comparative examples (Comparative Examples 1, 3, 5, etc.) in which the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is 4.0, at least when silver is used as the target material, the wear resistance of the silver-containing layer is evaluated as "×", and the result of the typing test is also evaluated as "×".
[0169] In addition, the surface covering materials for electric contacts obtained from comparative examples (Comparative Examples 2, 4, 6, etc.) in which the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) was 0.5 were evaluated as "×" at least in terms of bending workability.
[0170] Furthermore, among the examples of the present invention, the surface covering materials for electric contacts obtained from the examples in which the half-width of the peak derived from the Ag (111) plane was greater than 0.15° (Examples 1 to 14, 16, 18 to 33, 37 to 52, 54, and 56 of the present invention) were evaluated as "◎" for the wear resistance and typing test results of the silver-containing layer when silver was used as the target material. On the other hand, the surface covering materials for electric contacts obtained from the examples in which the half-width of the peak derived from the Ag (111) plane was less than 0.15° (Examples 15, 17, 34, 36, 53, and 55 of the present invention) were evaluated as "○" for the wear resistance and typing test results of the silver-containing layer when silver was used as the target material.
[0171] In addition, among the examples of the present invention, the bending workability of the surface covering materials for electric contacts obtained from the examples in which the half-width of the peak derived from the Ag (111) plane was less than 0.30° (Examples 1 to 13, 15, 17 to 32, 36 to 51, 53, and 55 of the present invention) was evaluated as "◎", while the bending workability of the surface covering materials for electric contacts obtained from the examples in which the half-width of the peak derived from the Ag (111) plane exceeded 0.30° (Examples 14, 16, 33, 35, 52, and 54 of the present invention) was evaluated as "○".
[0172] In addition, among the examples of the present invention, the contact resistance value of the surface covering material for electric contact obtained from the examples in which the content of the silver-containing layer was 99% by mass or more (Examples 1 to 11, 18 to 30, 37 to 49, 56, and 57 of the present invention) was evaluated as "◎", while the contact resistance value of the surface covering material for electric contact obtained from the examples in which the content of the silver-containing layer was less than 99% by mass (Examples 12 to 17, 31 to 36, and 50 to 55 of the present invention) was evaluated as "○".
[0173] In addition, among the examples of the present invention, the heat resistance of the surface covering material for electric contact obtained from the examples having the intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3 (Examples 20 to 57 of the present invention) was evaluated as "◎", while the heat resistance of the surface covering material for electric contact obtained from the examples having no intermediate layer 4 between the conductive substrate 2 and the silver-containing layer 3 (Examples 1 to 19 of the present invention) was evaluated as "○".
[0174] Reference numerals
[0175] 1,1A: Surface coating materials for electrical contacts
[0176] 2: Conductive substrate
[0177] 3: Silver-containing layer
[0178] 4: Middle layer
Claims
1. A surface coating material for an electric contact, comprising a conductive substrate and a silver-containing layer, wherein the silver-containing layer covers at least one side of the conductive substrate, wherein the surface coating material for an electric contact is characterized in that: When the first total peak intensity obtained from the X-ray diffraction pattern of the silver-containing layer is set to h1 and the second total peak intensity is set to h2, the ratio (h1 / h2) of the first total peak intensity (h1) to the second total peak intensity (h2) is in the range of greater than 1.0 and less than 3.0, the first total peak intensity is the total value of the peak intensity originating from the Ag (111) plane and the peak intensity originating from the plane parallel to the Ag (111) plane, and the second total peak intensity is the total value of the peak intensities remaining after subtracting the first total peak intensity (h1) from the total value of all detected peak intensities.
2. The surface covering material for an electric contact according to claim 1, wherein: In the silver-containing layer, the half width of a peak derived from the Ag (111) plane is in a range of 0.15° to 0.30°.
3. The surface covering material for an electric contact according to claim 1, wherein: The silver-containing layer contains 99 mass % or more of silver.
4. The surface covering material for an electric contact according to claim 1, wherein: The conductive substrate is made of pure copper, copper alloy, pure iron, iron alloy, pure aluminum or aluminum alloy.
5. The surface covering material for an electric contact according to claim 1, wherein: At least one intermediate layer is further provided between the conductive substrate and the silver-containing layer, and the intermediate layer is made of pure copper, copper alloy, pure nickel or nickel alloy.
6. The surface covering material for an electric contact according to claim 1, wherein: The conductive substrate has a thickness in a range of 0.03 mm to 0.30 mm.
7. An electric contact, which is produced by using the surface covering material for an electric contact according to any one of claims 1 to 6. A switch comprising the electric contact according to claim 7.
9. A connector terminal having the electric contact according to claim 7.