Low-temperature natural gas steam reforming hydrogen production catalyst as well as preparation method and application thereof
By using a low-temperature natural gas steam reforming hydrogen production catalyst in the natural gas steam reforming hydrogen production process, the problems of high energy consumption and serious carbon dioxide emissions in the high-temperature process are solved, high-efficiency hydrogen yield and carbon dioxide capture are achieved, and energy consumption and emission.
Patent Information
- Application Number
- CN202410776875.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
AI Technical Summary
The existing natural gas steam reforming hydrogen production process is carried out at high temperatures, resulting in high energy consumption and serious carbon dioxide emissions. The hydrogen volume fraction is low and cannot meet the needs of large-scale hydrogen production.
Using a low-temperature natural gas steam reforming hydrogen production catalyst, a mixed solution of inorganic silicon source, zirconium salt, cerium salt, praseodymium salt and calcium salt is prepared, olivine powder and inorganic alkali are added, and the co-precipitation reaction is carried out and then mixed with the chelating agent. Spray molding is used to prepare a "metal-alkaline" bifunctional molded catalyst for hydrogen production by natural gas steam reforming at low temperatures.
Achieve high methane conversion rate and high hydrogen yield at low temperature, reduce carbon deposition through hydrogen overflow, improve catalyst stability, and reduce reaction temperature through Le Chatelier's principle to achieve carbon dioxide capture and reuse, reduce carbon dioxide emissions and reduce energy consumption.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of natural gas resource utilization, and specifically relates to a low-temperature natural gas steam reforming hydrogen production catalyst and a preparation method and application thereof. Background Art
[0002] Energy is the material basis for the survival and development of human society and plays a vital role in the national economy. Modern energy pursues clean, efficient and pollution-free. Hydrogen energy has become one of the preferred targets for the next generation of green energy due to its high calorific value, clean products and large-scale production.
[0003] Natural gas hydrogen production technology is still the main method of hydrogen production due to its relatively low cost, accounting for 96% of the world's hydrogen production, and only 4% of hydrogen comes from water electrolysis. According to statistics, in 2020, the global production of hydrogen using natural gas accounted for 43.8%, and my country's hydrogen produced from natural gas accounted for 19% of the total annual hydrogen production.
[0004] The main methods of producing hydrogen from methane in industry include steam methane reforming (SMR), partial oxidation of methane (POM), and autothermal reforming of methane (ATR). The hydrogen production process in SMR is a traditional process that has been used in industry for more than 80 years. It has mature technology and simple reaction. Currently, 80% of the world's hydrogen is produced by this process, which is the lowest cost natural gas hydrogen production process. However, the SMR process is a strong endothermic reaction. The reaction requires high temperature, high energy consumption, and high requirements for reaction equipment. The hydrogen gas volume fraction obtained by the reaction is limited by the reaction balance and is less than 80%, and CO2 can only be discharged directly. SMR hydrogen production will emit 10-16 tons of carbon dioxide for every ton of hydrogen. This problem is particularly prominent today under the "dual carbon" situation.
[0005] SMR process technology fails to meet the requirements of large-scale hydrogen production. Therefore, researching and developing more advanced new natural gas hydrogen production process technologies is an important guarantee for solving the problem of cheap hydrogen sources. The new process technology should achieve breakthroughs in reducing carbon dioxide emissions and lowering energy consumption. Summary of the invention
[0006] The present invention is proposed to reduce carbon dioxide emissions and lower energy consumption for hydrogen production, and its purpose is to provide a low-temperature natural gas steam reforming hydrogen production catalyst and a preparation method and application thereof.
[0007] The present invention is achieved through the following technical solutions:
[0008] A method for preparing a catalyst for producing hydrogen by low-temperature natural gas steam reforming comprises the following steps:
[0009] (I) preparing a mixed solution of an inorganic silicon source, a zirconium salt, a cerium salt, a praseodymium salt and a calcium salt, and adding olivine powder to the mixed solution to obtain a suspension;
[0010] (II) adding an inorganic alkali solution to the suspension obtained in step (I) to make the pH value of the suspension be 12 to 14, stirring, performing a coprecipitation reaction, and then washing and filtering to obtain a composite metal oxide carrier;
[0011] (III) mixing the composite metal oxide support obtained in step (II) with a chelating agent solution, and then adding metal ions to obtain a catalyst raw powder solution;
[0012] (IV) The catalyst raw powder solution is sprayed into a mold to obtain a low-temperature natural gas steam reforming hydrogen production catalyst.
[0013] In the above technical scheme, the inorganic silicon source is any one of water glass or silica sol; the zirconium salt is any one or more of zirconium nitrate, zirconium sulfate, zirconium chloride, zirconium fluoride, zirconium oxalate, zirconium citrate or zirconium methacrylate; the cerium salt is any one or more of cerium nitrate, cerium sulfate, cerium chloride, cerium acetate or cerium oxalate; the praseodymium salt is any one or more of praseodymium nitrate, praseodymium sulfate, praseodymium chloride, praseodymium acetate, praseodymium carbonate or praseodymium oxalate; the calcium salt is any one or more of calcium nitrate, calcium sulfate, calcium chloride, calcium acetate or calcium oxalate.
[0014] In the above technical solution, the molar ratio of the inorganic silicon source, zirconium salt, cerium salt, praseodymium salt and calcium salt in the mixed solution is 15:2:2:1:80; the concentration of zirconium salt in the mixed solution is 0.01 mol·L -1 ~0.1mol·L -1 .
[0015] In the above technical solution, the solid-liquid mass ratio of the olivine powder to the mixed solution is 1:(5-10).
[0016] In the above technical solution, the inorganic base is any one or a combination of two of lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium carbonate or ammonia water.
[0017] In the above technical solution, the concentration of the inorganic base in the suspension is 0.5 mol / L to 10 mol / L.
[0018] In the above technical solution, the temperature of the coprecipitation reaction in step (II) is 25°C to 150°C, and the reaction time is 2h to 10h.
[0019] In the above technical scheme, the chelating agent in step (III) is any one or more of ketoxime, carboxylic acid or amine; the solid-liquid mass ratio of the composite metal oxide support to the chelating agent solution in step (III) is 1:(5-10); the concentration of the chelating agent solution in step (III) is 0.5 mol·L -1 ~5mol·L -1 ; The concentration of the metal salt solution in step (III) is 1wt% to 10wt%.
[0020] In the above technical scheme, the volumes of the chelating agent solution and the metal salt solution in step (III) are the same, that is, 100 mL of the chelating agent solution is taken to dissolve the composite metal oxide carrier, and then 100 mL of the metal salt solution with a concentration of 0.005 to 0.5 molL-1 is mixed evenly to obtain a metal salt-modified catalyst raw powder solution.
[0021] In the above technical solution, the metal ions of the metal salt solution in step (III) are any one or more combinations of Ni, Co, Zn, Mo, Fe, Pt, Ru, or Ga.
[0022] In the above technical scheme, the specific method of drying in step (IV) is: drying the spray-formed catalyst at 110°C overnight; the specific method of calcining is: heating from room temperature to 100°C at a heating rate of 2°C / min, staying at 100°C for 60 minutes, then heating from 100°C to 200°C at a heating rate of 2°C / min, staying at 200°C for 60 minutes, then heating to 600°C according to the heating method, then keeping the temperature constant for 6 hours and then starting to cool naturally, and when the temperature is cooled to room temperature, a binder-free natural gas steam reforming hydrogen production formed catalyst is obtained.
[0023] A low-temperature natural gas steam reforming hydrogen production catalyst is prepared by the above method.
[0024] Application of a low-temperature natural gas steam reforming hydrogen production catalyst in a low-temperature natural gas steam reforming hydrogen production reaction, wherein the low-temperature natural gas steam reforming hydrogen production reaction adopts a fixed bed process, the low-temperature reaction temperature is 450°C to 600°C, the reaction pressure is 0 to 1MPa, and the space velocity is 1000h -1 ~18000h -1 .
[0025] The beneficial effects of the present invention are:
[0026] The present invention provides a low-temperature natural gas steam reforming hydrogen production catalyst and a preparation method and application thereof. The prepared integrated "metal-alkaline" bifunctional formed catalyst can carry out natural gas steam reforming hydrogen production reaction at low temperature (≤600°C), and has the characteristics of high methane conversion rate and high hydrogen yield; a hydroxylated surface is formed on the catalyst, and the formation of carbon deposits is reduced by hydrogen overflow, thereby improving the stability of the catalyst; at the same time, through the Le Chatelier principle, the chemical equilibrium is broken, the reaction temperature of natural gas steam reforming hydrogen production is reduced, and the hydrogen yield is improved; while the catalyst produces hydrogen, it can in-situ reversibly chemically absorb carbon dioxide generated in the reaction process, and the carbon dioxide absorbed in the reaction process can be captured and reused in subsequent catalyst regeneration, thereby realizing CO2 capture and release at medium and low temperatures, and achieving breakthroughs in reducing carbon dioxide emissions and reducing energy consumption; the preparation method has simple steps, readily available raw materials, energy saving and consumption reduction, and has certain industrial application potential. DETAILED DESCRIPTION
[0027] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention is further described below through specific implementation methods.
[0028] Example 1
[0029] A method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming, comprising the following steps:
[0030] (i) preparing a mixed solution of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate, wherein the molar ratio of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80, adding crushed olivine powder to the mixed solution to obtain a suspension; the solid-liquid ratio of the olivine powder to the mixed solution is 1:5; the concentration of the zirconium salt in the mixed solution is 0.05 mol·L -1 ;
[0031] (ii) adding a 10% NaOH solution to the suspension obtained in step (I) to make the pH value of the suspension 12, stirring at 90° C. for 4 h to carry out a coprecipitation reaction, and then washing and filtering to obtain an alkaline composite metal oxide carrier;
[0032] (iii) At room temperature, the alkaline composite metal oxide support obtained in step (II) was mixed with ethylenediamine at a solid-liquid mass ratio of 1:5. 100 mL of the mixed solution of the composite metal oxide support and the chelating agent solution (ethylenediamine solution) was taken, and then 100 mL of the mixed metal salt solution was added thereto for chelation. The concentration of the ethylenediamine solution was 4 mol·L -1The mass fraction of Ni salt in the mixed metal salt solution is 10%, the mass fraction of Co salt is 10%, and the mass fraction of Pt salt is 1%. After complexation, the above-mentioned natural gas steam reforming hydrogen production catalyst raw powder solution is obtained;
[0033] (iv) directly spraying the catalyst raw powder solution into a mold to obtain the catalyst;
[0034] (v) The catalyst was transferred to an oven and dried at 110°C overnight, then transferred to a muffle furnace, and the temperature was increased from room temperature to 100°C at a heating rate of 2°C / min, and the temperature was kept at 100°C for 60 minutes. Then, the temperature was increased from 100°C to 200°C at a heating rate of 2°C / min, and the temperature was kept at 200°C for 60 minutes. Thereafter, the temperature was increased to 600°C according to the heating method, and then the temperature was kept constant for 6 hours and then naturally cooled. When the temperature was cooled to room temperature, a binder-free natural gas steam reforming hydrogen production catalyst was obtained.
[0035] Example 2
[0036] The difference from Example 1 is that in step (i), the silicon source is replaced with water glass, and a mixed solution of water glass, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate is prepared, the molar ratio of water glass, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80, and crushed olivine powder is added to the mixed solution to obtain a suspension; the solid-liquid ratio of olivine powder to the mixed solution is 1:5.
[0037] Example 3 (without introduction of olivine)
[0038] A method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming, comprising the following steps:
[0039] (i) preparing a mixed solution of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate, wherein the molar ratio of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80;
[0040] (ii) adding a 10% NaOH solution to the mixed solution obtained in step (I) to make the pH value of the suspension 12, stirring at 90° C. for 4 h to carry out a coprecipitation reaction, and then washing and filtering to obtain an alkaline composite metal oxide carrier;
[0041] (iii) at room temperature, the composite metal oxide support obtained in step (II) was mixed with ethylenediamine at a solid-liquid ratio of 1:5, and then metal ions of 10% Ni salt ethylenediamine solution, 10% Co salt ethylenediamine solution and 1% Pt salt ethylenediamine solution were introduced for complexation to obtain the above-mentioned natural gas steam reforming hydrogen production catalyst raw powder solution;
[0042] (iv) directly spraying the catalyst raw powder solution into a mold to obtain the catalyst;
[0043] (v) The catalyst was transferred to an oven and dried at 110°C overnight, then transferred to a muffle furnace, and heated from room temperature to 100°C at a heating rate of 2°C / min, and kept at 100°C for 1 hour. Then, the temperature was increased from 100°C to 200°C at a heating rate of 2°C / min, and kept at 200°C for 1 hour. Thereafter, the temperature was increased to 600°C according to the heating method, and then the temperature was kept constant for 6 hours and then naturally cooled. When the temperature was cooled to room temperature, a binder-free natural gas steam reforming hydrogen production catalyst was obtained.
[0044] Example 4
[0045] The difference from Example 1 is that the solid-liquid ratio of the olivine powder to the mixed solution in step (i) is adjusted, and a mixed solution of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate is prepared, the molar ratio of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80, and the crushed olivine powder is added to the mixed solution to obtain a suspension; the solid-liquid ratio of the olivine powder to the mixed solution is 1:10.
[0046] Example 5
[0047] The difference from Example 1 is that in the adjustment step (iii), the alkaline composite metal oxide support obtained in step (ii) is first dried at 110°C, calcined at 540°C for 4h, cooled to room temperature, and then mixed with ethylenediamine at a solid-liquid ratio of 1:5 to prepare a natural gas steam reforming hydrogen production catalyst raw powder solution.
[0048] Example 6
[0049] The difference from Example 1 is that the mixing ratio of the composite metal oxide support and ethylenediamine in step (iii) is changed to a solid-liquid ratio of 1:10, and then metal ions with mass fractions of 10% Ni, 10% Co and 1% Pt are introduced for complexation to obtain the above-mentioned natural gas steam reforming hydrogen production catalyst raw powder solution.
[0050] Example 7
[0051] The difference from Example 1 is that the praseodymium nitrate in the mixed solution prepared in step (i) is replaced by yttrium nitrate, and the molar ratio of silica sol, zirconium nitrate, cerium nitrate, yttrium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80.
[0052] Example 8
[0053] A method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming, comprising the following steps:
[0054] (i) preparing a mixed solution of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate, wherein the molar ratio of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80, adding crushed olivine powder to the mixed solution to obtain a suspension; the solid-liquid ratio of the olivine powder to the mixed solution is 1:5; the concentration of the zirconium salt in the mixed solution is 0.05 mol·L -1 ;
[0055] (ii) adding a 10% NaOH solution to the suspension obtained in step (I) to make the pH value of the suspension 12, stirring at 90° C. for 4 h to carry out a coprecipitation reaction, and then washing and filtering to obtain an alkaline composite metal oxide carrier;
[0056] (iii) at room temperature, the composite metal oxide support obtained in step (II) was mixed with ethylenediamine at a solid-liquid mass ratio of 1:10, and then 10% by mass of Ni metal ions were introduced for complexation to obtain the above-mentioned natural gas steam reforming hydrogen production catalyst raw powder solution;
[0057] (iv) The catalyst raw powder solution is directly sprayed into a mold to obtain the catalyst.
[0058] Example 9
[0059] A method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming, comprising the following steps:
[0060] (i) preparing a mixed solution of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate, wherein the molar ratio of silica sol, zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 15:2:2:1:80, adding crushed olivine powder to the mixed solution to obtain a suspension; the solid-liquid ratio of the olivine powder to the mixed solution is 1:5; the concentration of the zirconium salt in the mixed solution is 0.05 mol·L -1 ;
[0061] (ii) adding a 10% NaOH solution to the suspension obtained in step (I) to make the pH value of the suspension 12, stirring at 90° C. for 4 h to carry out a coprecipitation reaction, and then washing and filtering to obtain an alkaline composite metal oxide carrier;
[0062] (iii) at room temperature, the composite metal oxide support obtained in step (II) was mixed with ethylenediamine at a solid-liquid ratio of 1:10, and then 10% by mass of Ni and 10% by mass of Co metal ions were introduced for complexation to obtain the above-mentioned natural gas steam reforming hydrogen production catalyst raw powder solution;
[0063] (iv) The catalyst raw powder solution is directly sprayed into a mold to obtain the catalyst.
[0064] Comparative Example 1
[0065] A method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming, comprising the following steps:
[0066] (i) preparing a mixed solution of zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate, wherein the molar ratio of zirconium nitrate, cerium nitrate, praseodymium nitrate and calcium nitrate in the mixed solution is 2:2:1:80; and the concentration of zirconium salt in the mixed solution is 0.05 mol·L -1 ;
[0067] (ii) adding a 10% NaOH solution to the mixed solution obtained in step (I) at room temperature to make the pH value of the suspension 12, stirring at 90° C. for 4 h to carry out a coprecipitation reaction, and then washing and filtering to obtain an alkaline composite metal oxide carrier;
[0068] (iii) slurrying the composite metal oxide carrier obtained in step (II) with silica sol at a solid-liquid ratio of 1:10, wherein the SiO2 content in the silica sol is 10%, and then directly spraying and molding, drying at 110°C overnight, and calcining at 750°C for 4h to obtain a basic composite metal oxide molded carrier;
[0069] (iv) The formed composite metal oxide is used as a carrier, and metal loadings of 10% Ni, 10% Co and 1% Pt are performed, respectively. The catalyst is then filtered, dried at 110°C, and calcined at 540°C for 4h to obtain a formed catalyst for hydrogen production from steam reforming of natural gas.
[0070] Catalyst performance evaluation:
[0071] It was carried out on a 20mL adiabatic micro fixed bed reactor. 1g of the catalyst prepared in Examples 1-9 and Comparative Example 1 was weighed and mixed with 5mL of quartz sand and then loaded into the constant temperature section of the reaction tube. Quartz sand and quartz wool were used to fill both ends. Nitrogen was continuously introduced during the programmed temperature rise process. It was stabilized at 300°C and 450°C for 20min respectively. After heating to the required reaction temperature of 600°C, it was maintained for 30min to activate the catalyst and then the reaction gas was introduced. The feed volume ratio of methane and water vapor was 1:4, the anti-methane flow rate was 20mL / min, the water pump speed was 0.064mL / min, the carrier gas nitrogen was 30mL / min, and the reaction pressure was 3MPa. Analysis was started 30min after the reaction started to ensure that the reaction started to run stably. After that, product analysis was performed using online gas chromatography every 1h. The experimental results are shown in Table 1 below:
[0072] Table 1: Experimental results of catalytic performance of various catalysts under the same reaction conditions
[0073]
[0074] From the reaction results, under the same reaction conditions, the catalysts used in Examples 1-9 can achieve a CH4 conversion rate of more than 80% and a H2 yield of more than 70%, and the reaction performance is good. However, the catalyst used in Comparative Example 1 has a poor reaction effect, with a CH4 conversion rate of only 35% and a H2 yield of 33%. Therefore, the "metal-alkaline" bifunctional binder-free formed catalysts prepared in Examples 1-9 have obvious reaction activity advantages.
[0075] The present invention first synthesizes an alkaline composite metal oxide carrier, then introduces a metal active component through a chelation method to obtain a catalyst raw powder solution, and finally directly sprays and molds the catalyst. The "metal-alkaline" bifunctional molded catalyst prepared by the present invention with an alkaline mineral composite metal oxide as a carrier can produce hydrogen while adsorbing carbon dioxide generated during the reaction. Through the Le Chatelier principle, the chemical equilibrium is broken, the reaction temperature of natural gas steam reforming hydrogen production is reduced, and the yield of hydrogen is increased. The carbon dioxide absorbed during the reaction can also be captured and reused in subsequent catalyst regeneration, achieving breakthroughs in reducing carbon dioxide emissions and reducing energy consumption.
[0076] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming, characterized in that: The following steps are involved: (I) preparing a mixed solution of an inorganic silicon source, a zirconium salt, a cerium salt, a praseodymium salt and a calcium salt, and adding olivine powder to the mixed solution to obtain a suspension; (II) adding an inorganic alkali solution to the suspension obtained in step (I) to make the pH value of the suspension be 12 to 14, stirring, performing a coprecipitation reaction, and then washing and filtering to obtain a composite metal oxide carrier; (III) mixing the composite metal oxide support obtained in step (II) with a chelating agent solution, and then adding a metal salt solution to obtain a catalyst raw powder solution; (IV) The catalyst raw powder solution is sprayed into shape, and after drying and calcining, a low-temperature natural gas steam reforming hydrogen production catalyst is obtained.
2. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: The inorganic silicon source is any one of water glass or silica sol; the zirconium salt is any one or more of zirconium nitrate, zirconium sulfate, zirconium chloride, zirconium fluoride, zirconium oxalate, zirconium citrate or zirconium methacrylate; the cerium salt is any one or more of cerium nitrate, cerium sulfate, cerium chloride, cerium acetate or cerium oxalate; the praseodymium salt is any one or more of praseodymium nitrate, praseodymium sulfate, praseodymium chloride, praseodymium acetate, praseodymium carbonate or praseodymium oxalate; the calcium salt is any one or more of calcium nitrate, calcium sulfate, calcium chloride, calcium acetate or calcium oxalate; the molar ratio of the inorganic silicon source, zirconium salt, cerium salt, praseodymium salt and calcium salt in the mixed solution is 15:2:2:1:80; the concentration of the zirconium salt in the mixed solution is 0.01 mol·L -1 ~0.1mol·L -1 .
3. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: In the step (I), the solid-liquid mass ratio of the olivine powder to the mixed solution is 1:(5-10).
4. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: The inorganic base is any one of lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium carbonate or ammonia water, or a combination of two thereof.
5. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: The temperature of the coprecipitation reaction in step (II) is 25° C. to 150° C., and the reaction time is 2 h to 10 h.
6. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: The chelating agent in step (III) is any one or more of ketoxime, carboxylic acid or amine; the solid-liquid mass ratio of the composite metal oxide support to the chelating agent solution in step (III) is 1:(5-10); the concentration of the chelating agent solution in step (III) is 0.5 mol·L -1 ~5mol·L -1 ; The concentration of the metal salt solution in step (III) is 1wt% to 10wt%.
7. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: The metal ions of the metal salt solution in step (III) are any one or more combinations of Ni, Co, Zn, Mo, Fe, Pt, Ru, or Ga.
8. The method for preparing a catalyst for hydrogen production by low-temperature natural gas steam reforming according to claim 1, characterized in that: The specific method of drying in step (IV) is: drying the spray-formed catalyst at 110°C overnight; the specific method of calcining is: heating from room temperature to 100°C at a heating rate of 2°C / min, staying at 100°C for 60 minutes, then heating from 100°C to 200°C at a heating rate of 2°C / min, staying at 200°C for 60 minutes, then heating to 600°C according to the heating method, then keeping the temperature constant for 6 hours and then starting to cool naturally, and when the temperature is cooled to room temperature, a binder-free natural gas steam reforming hydrogen production formed catalyst is obtained.
9. A low-temperature natural gas steam reforming hydrogen production catalyst, characterized in that: Prepared by the method according to any one of claims 1 to 7.
10. An application of the method according to any one of claims 1 to 8 in preparing a catalyst for low-temperature natural gas steam reforming hydrogen production, characterized in that: The natural gas steam reforming hydrogen production catalyst is used for low-temperature natural gas steam reforming hydrogen production reaction; the low-temperature natural gas steam reforming hydrogen production reaction adopts a fixed bed process, the low-temperature reaction temperature is 450°C to 600°C, the reaction pressure is 0 to 1MPa, and the space velocity is 1000h -1 ~18000h -1 .
Citation Information
Patent Citations
Catalyst for preparing hydrogen-rich gas by coke oven gas and preparation method thereof
CN101181685A
Catalyst for hydrogen production from methane vapor reforming and preparing method thereof
CN101224427A
Moulding olivine nickel-loaded catalyst and preparation method thereof
CN101332429A
Catalyst for hydrogen production by bio-oil steam reforming and preparation method thereof
CN101444740A
Preparation method and application of catalyst composition for hydrocarbon Fischer-Tropsch synthesis
CN105817222A
Cited By
In-situ carbon capture and conversion method based on three-way catalyst
CN119346120A