A galena assemblage inhibitor and its application
By combining the oxidation and adsorption effects of inhibitors, the problem of low separation efficiency between chalcopyrite and galena is solved, achieving efficient and environmentally friendly flotation separation, adapting to a wide pH range, and allowing for the reuse of filtrate.
Patent Information
- Application Number
- CN202410909993.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-07-08
AI Technical Summary
In existing technologies, the flotation separation efficiency of chalcopyrite and galena is low, and the concentrate grade and recovery rate are low. Conventional reagents such as potassium permanganate pose significant environmental hazards, and enterprises urgently need efficient and environmentally friendly inhibitors.
A combination of inhibitors, including perbromic acid, salicylic acid, and D-erythrose, is used to reduce the hydrophobicity of the galena surface through oxidation and chemical and physical adsorption, thereby achieving effective separation of chalcopyrite and galena.
It improves the recovery rate of chalcopyrite and reduces the recovery rate of galena. The combined inhibitor is environmentally friendly and non-toxic, adaptable to a wide pH range, does not require heating, and the filtrate can be reused.
Smart Images

Figure CN118788492B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a galena composite inhibitor and its application, belonging to the field of mineral processing technology. Background Technology
[0002] Copper and lead are common non-ferrous metal raw materials that play a crucial role in national economic development. However, the massive consumption of copper and lead resources necessitates strengthened research into their utilization. This makes the utilization of low-grade complex ores increasingly important. The development and utilization of such ores is a complex process that may cause serious environmental and economic problems.
[0003] Chalcopyrite is a major copper mineral, often associated with galena. Chalcopyrite and galena have very similar floatability, and their flotation separation in copper-lead sulfide ores often suffers from low separation efficiency, low concentrate grade, and low recovery. With the depletion of high-grade, easily separable sulfide ore resources, researchers have begun to focus on the utilization of copper and lead resources in low-grade, difficult-to-process sulfide ores, posing increasingly stringent challenges and experiments to the flotation separation of copper and lead sulfide ores. The difficulty in separating copper-lead sulfide ores is a common problem in current production. An effective way to improve the flotation separation of chalcopyrite and galena lies in developing efficient inhibitor systems.
[0004] Conventional flotation processes use strong oxidants and potassium permanganate to selectively inhibit galena, making its surface hydrophilic. Then, collectors are used to float chalcopyrite, achieving separation between the two. However, conventional reagents like potassium permanganate pose significant environmental hazards and their use is subject to many restrictions. Therefore, companies urgently need highly effective depressants. Summary of the Invention
[0005] In order to solve the problems existing in the existing galena inhibitors, one of the objectives of the present invention is to provide a galena composite inhibitor, wherein the composite inhibitor comprises, by mass percentage: 10% to 40% perbromic acid, 20% to 40% salicylic acid, and 40% to 80% D-erythrose.
[0006] Another object of the present invention is to provide an application of a galena composite inhibitor in the flotation separation of galena and chalcopyrite.
[0007] Preferably, the dosage of the combined inhibitor in the flotation separation process is 100-400 g / t. When using it, perbromic acid is added first for reaction and filtration, and then salicylic acid and D-erythrose are added.
[0008] Preferably, the flotation separation specifically includes the following steps:
[0009] (1) Now add perbromic acid to the raw slurry, react and filter, then add salicylic acid and D-erythrose, and filter to obtain a slurry mixture.
[0010] (2) Add a frother and a collector to the slurry mixture obtained in step (1), and obtain lead concentrate through a single roughing process. The tailings are copper concentrate. Preferably, the pH of the original slurry in step (1) is 5 to 11.
[0011] Preferably, in step (2), the foaming agent is pine oil, and the dosage is 15g / t; the collector is ethyl xanthate, and the dosage is 20g / t.
[0012] The principle of this invention: Perbromic acid is an oxidizing agent that can oxidize the surface of galena, generating PbO and PbSO4 oxides. These oxides are hydrophilic species, which can reduce the hydrophobicity of the galena surface. The carboxyl group of salicylic acid can react with lead on the oxidized galena surface, while the hydroxyl group of salicylic acid has difficulty reacting with lead. Therefore, the adsorption of salicylic acid also leads to the hydrophilicity of the galena surface. D-erythrose contains multiple hydroxyl groups, which can form hydrogen-bond-like interactions with oxygen atoms on the oxidized galena surface, thus adsorbing onto the galena surface and further forming a hydrophilic surface. Therefore, the combined agent, through the oxidation of sulfur atoms in galena by HBrO4, the chemisorption of salicylic acid at lead sites, and the physisorption of D-erythrose, produces a significant synergistic effect, effectively reducing the hydrophobicity of the galena surface and thus producing an inhibitory effect.
[0013] Beneficial effects of the present invention
[0014] (1) The combined inhibitors shown in this invention are used to separate galena and chalcopyrite by flotation, wherein the recovery rate of galena is only 8% to 10%, while the recovery rate of chalcopyrite is 85% to 90%.
[0015] (2) The combination inhibitor of the present invention is green, safe, environmentally friendly and non-toxic, easy to use, and has strong selective inhibition, which solves the problem of slurry sedimentation, and also overcomes the problem of low final copper-lead separation efficiency caused by the forced inhibition of fine lead minerals.
[0016] (3) In the process of using the combined inhibitor of the present invention, there is no need to heat the slurry. It can produce a strong inhibitory effect on galvanite at room temperature of 25°C. Moreover, the combined inhibitor can adapt to a wide pH range of pH=5-11.
[0017] (4) The combined inhibitors described in this invention can be reused after filtration. Attached Figure Description
[0018] Figure 1 The molecular formula of D-erythrose used in this invention is shown below.
[0019] Figure 2 The molecular formula of salicylic acid used in this invention is given.
[0020] Figure 3This is a flow chart of the flotation process used in this invention. Detailed Implementation
[0021] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments. However, the following embodiments are merely simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention is determined by the claims.
[0022] Example 1
[0023] The raw ore used in this embodiment comes from Kunming City, Yunnan Province. The amount of the combined inhibitor used in this embodiment is 300g / t, of which the mass of perbromic acid is 10%, the mass of salicylic acid is 40%, and the mass of D-erythrose is 50%.
[0024] A flotation separation method for galena and chalcopyrite, the specific steps of which are as follows:
[0025] (1) Add raw ore slurry to the mixing tank. The pH of the slurry is 5. First add perbromic acid and react for 20 minutes. After filtration, add salicylic acid and D-erythrose and react for 20 minutes. Filter again to obtain the slurry mixture. The filtrate obtained from the two filtrations in this step can be reused 3 times.
[0026] (2) Water is added to the slurry mixture obtained in step (1), 15g / t of pine oil is added as a foaming agent, and 20g / t of ethyl xanthate is used as a collector. Lead concentrate is obtained through one roughing process, and the tailings are copper concentrate.
[0027] The test results showed that the copper concentrate had a copper grade of 20.46% and a copper recovery rate of 87.88%, and contained 3.89% lead.
[0028] Example 2
[0029] The raw ore used in this embodiment comes from Kunming City, Yunnan Province. The amount of the combined inhibitor used in this embodiment is 100g / t, of which the mass of perbromic acid is 40%, the mass of salicylic acid is 20%, and the mass of D-erythrose is 40%.
[0030] A flotation separation method for galena and chalcopyrite, the specific steps of which are as follows:
[0031] (1) Add raw ore slurry to the mixing tank. The pH of the slurry is 8. First add perbromic acid and react for 20 minutes. After filtration, add salicylic acid and D-erythrose and react for 20 minutes. Filter again to obtain the slurry mixture. The filtrate obtained from the two filtrations in this step can be reused 3 times.
[0032] (2) Water is added to the slurry mixture obtained in step (1), 15g / t of pine oil is added as a foaming agent, and 20g / t of ethyl xanthate is used as a collector. Lead concentrate is obtained through one roughing process, and the tailings are copper concentrate.
[0033] The test results showed that the copper concentrate had a copper grade of 19.67% and a copper recovery rate of 88.10%, and contained 4.05% lead.
[0034] Example 3
[0035] The raw ore used in this embodiment comes from Kunming City, Yunnan Province. The amount of the combined inhibitor used in this embodiment is 400g / t, of which the mass of perbromic acid is 10%, the mass of salicylic acid is 40%, and the mass of D-erythrose is 50%.
[0036] A flotation separation method for galena and chalcopyrite, the specific steps of which are as follows:
[0037] (1) Add raw ore slurry to the mixing tank. The pH of the slurry is 11. First add perbromic acid and react for 20 minutes. After filtration, add salicylic acid and D-erythrose and react for 20 minutes. Filter again to obtain the slurry mixture. The filtrate obtained from the two filtrations in this step can be reused 3 times.
[0038] (2) Water is added to the slurry mixture obtained in step (1), 15g / t of pine oil is added as a foaming agent, and 20g / t of ethyl xanthate is used as a collector. Lead concentrate is obtained through one roughing process, and the tailings are copper concentrate.
[0039] The test results showed that the copper concentrate had a copper grade of 20.33% and a copper recovery rate of 88.03%, and contained 3.951% lead.
[0040] Comparative Example 1
[0041] In comparison, the only difference between this comparative example and Example 1 is that the inhibitor used is perbromic acid, and the flotation of the raw ore and the flotation separation method are the same as in Example 1.
[0042] The test results showed that the copper concentrate had a copper grade of 15.45% and a copper recovery rate of 67.77%, and contained 15.43% lead. Since the inhibitor described was a single perbromic acid, compared to Example 1, it lacked the synergistic effect of salicylic acid and D-erythrose, and the oxidation effect of perbromic acid alone was insufficient to fully inhibit galena.
[0043] Comparative Example 2
[0044] In comparison, the only difference between this comparative example and Example 1 is that the inhibitor used is salicylic acid, and the flotation of the raw ore and the flotation separation method are the same as in Example 1.
[0045] The test results showed that the copper concentrate with a copper grade of 14.85% and a copper recovery rate of 50.58% contained 14.67% lead. Although salicylic acid can be adsorbed on the surface of galena, its adsorption alone is far from sufficient to inhibit galena, and therefore cannot fully inhibit galena.
[0046] Comparative Example 3
[0047] In comparison, the only difference between this comparative example and Example 1 is that the inhibitor used is D-erythrose, and the flotation of the raw ore and the flotation separation method are the same as in Example 1.
[0048] The experimental results showed that the copper concentrate with a copper grade of 17.20% and a copper recovery rate of 71.67% contained 10.67% lead. D-erythrose contains multiple hydroxyl groups, which can form hydrogen-like bonds with oxygen atoms on the surface of oxidized galena, thus adsorbing onto the galena surface and further forming a hydrophilic surface. However, at the current dosage, relying solely on this single agent is far from sufficient to fully inhibit galena.
[0049] Comparative Example 4
[0050] In comparison, the only difference between this comparative example and Example 1 is that the inhibitors used include 50% perbromic acid and 50% salicylic acid, and the flotation of the raw ore and the flotation separation method are the same as in Example 1.
[0051] The experimental results showed that the copper concentrate had a copper grade of 16.89% and a copper recovery rate of 69.46%, and contained 14.33% lead. The results also indicated that perbromic acid and salicylic acid could produce a small synergistic effect, but this was significantly less than the synergistic effect of perbromic acid, salicylic acid, and D-erythrose.
[0052] Comparative Example 5
[0053] In comparison, the only difference between this comparative example and Example 1 is that the inhibitors used include 50% perbromic acid and 50% D-erythrose, and the flotation of the raw ore and the flotation separation method are the same as in Example 1.
[0054] The experimental results showed that the copper concentrate had a copper grade of 18.53% and a copper recovery rate of 75.01%, with a lead content of 9.19%. The results also indicated that perbromic acid and D-erythrose could produce a small synergistic effect, but this was still significantly less than the synergistic effect of perbromic acid, salicylic acid, and D-erythrose.
[0055] Comparative Example 6
[0056] In comparison, the only difference between this comparative example and Example 1 is that the inhibitors used include 50% salicylic acid and 50% D-erythrose, and the flotation of the raw ore and the flotation separation method are the same as in Example 1.
[0057] The experimental results showed that the copper concentrate had a copper grade of 18.11% and a copper recovery rate of 74.87%, with a lead content of 9.55%. The results also indicated that salicylic acid and D-erythrose could produce a small synergistic effect, but this was significantly less than the synergistic effect of perbromic acid, salicylic acid, and D-erythrose as a whole.
Claims
1. The application of a galena composite depressant in the flotation separation of galena and chalcopyrite, characterized in that: The combined inhibitor comprises, by mass percentage: 10%~40% perbromic acid, 20%~40% salicylic acid, and 40%~50% D-erythrose. The amount of the combined inhibitor used in the flotation separation process is 100~400g / t. When using it, perbromic acid is added first for reaction and filtration, and then salicylic acid and D-erythrose are added.
2. The application of the galena composite depressant according to claim 1 in the flotation separation of galena and chalcopyrite, characterized in that: The flotation separation steps are as follows: (1) First, add perbromic acid to the raw slurry, react and filter, then add salicylic acid and D-erythrose, and filter to obtain a slurry mixture; (2) Add frother and collector to the slurry mixture obtained in step (1), and obtain lead concentrate through one roughing process. The tailings are copper concentrate.
3. The application of the galena composite depressant according to claim 2 in the flotation separation of galena and chalcopyrite, characterized in that: In step (1), the pH of the raw ore slurry is 5-11.
4. The application of the galena composite depressant according to claim 2 in the flotation separation of galena and chalcopyrite, characterized in that: In step (2), the foaming agent is pine oil, and the dosage is 15g / t; the collector is ethyl xanthate, and the dosage is 20g / t.
Citation Information
Patent Citations
A Flotation Process
AU2012203702A1
Beneficiation method for copper-lead sulphide ore
CN108405189A