Method for polishing and improving finish degree of small table top based on high-pressure SiC anvil cell

By using a mixed polishing paste of diamond powder, aluminum powder and olive oil, combined with mechanical polishing of cast iron discs, the problem of substandard polishing finish of SiC anvils was solved, achieving efficient polishing improvement, meeting the needs of high-pressure physics research, and simplifying process and increased yield.

CN118789367AActive Publication Date: 2024-10-18JIPA TECHNOLOGY (SHENZHEN) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411168730.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-10-18
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The polishing finish of domestic SiC anvils is not up to standard, resulting in poor parallelism and easy chipping or cracking, which affects the pressure value of high-pressure physics research and the needs of scientific research. Moreover, traditional diamond powder processing results in black stripes, which is difficult to meet the requirements of scientific research.

Method used

Using a mixed polishing paste of diamond powder, aluminum powder and olive oil, through mechanical polishing of the cast iron plate, adjusting the polishing material proportion and steps, including stirring, standing, even application and multiple polishing, combined with preheating treatment and cleaning detection, to improve The finish of the SiC anvil.

Benefits of technology

The polishing effect of the SiC anvil is significantly improved, scratches and black streaks are avoided, the finish requirements of scientific research are met, the yield and processing efficiency are increased, the process is simplified, and it is suitable for existing production conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789367A_ABST
    Figure CN118789367A_ABST
Patent Text Reader

Abstract

The invention discloses a method for polishing and improving the finish degree of a small table top of a SiC anvil for high pressure, which comprises the following steps of: preparing a polishing material which comprises diamond powder, aluminum powder and olive oil; uniformly mixing the diamond powder with olive oil, stirring into a thick state, and standing for a period of time; adding aluminum powder into the mixture, continuously stirring uniformly, and standing for a period of time; and uniformly smearing the mixed polishing paste on a cast iron disc, then uniformly distributing the polishing paste on the surface of the cast iron disc by using a disc pushing stone turning arm, and polishing the small table top of the SiC anvil cell by using the polishing paste so as to improve the smoothness of the table top. By optimizing the components and proportion of the polishing powder, the smoothness of the small table top of the SiC anvil for high pressure is effectively improved, and the problem that black stripes and scratches are easily generated in the polishing process in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of processing SiC anvils used in high-pressure experiments, and in particular to a method for polishing and improving the finish of a small table of a SiC anvil used for high pressure. Background Art

[0002] SiC anvils have very important applications in the field of high-pressure physics research. Compared with diamond anvils, SiC anvils are more affordable. Raman spectroscopy can be used to test the relevant signals in the 1332.5 region of the diamond anvil Raman characteristic peak, which is of great significance for scientific research. At present, SiC anvils used in domestic high-pressure physics research mainly rely on foreign imports, with long supply cycles, high prices, inconvenient maintenance and after-sales service, and the finish does not meet the ideal requirements; domestic manufacturers produce SiC anvils, and the polishing finish does not meet the ideal requirements, resulting in a pair of anvils being poorly parallel during use. Once pressurized, they will collapse or crack, and the expected pressure value cannot be achieved, which has a great impact on the corresponding scientific research; At present, the traditional diamond powder is used in the processing of SiC in China, which will cause poor polishing during processing and black stripes on the polished surface, which is difficult to meet the requirements of scientific research.

[0003] like Figure 1 As shown, the current SiC anvil processing is mainly based on the way and method of diamond processing. The polishing uses mechanical polishing with a cast iron disk and diamond powder. Since the Mohs hardness of SiC itself is 9.5 and the Mohs hardness of diamond powder is 10, and since diamond powder is harder than SiC, the sample will be constantly scratched during mechanical polishing, resulting in black lines, which will have a great impact on polishing and cannot produce samples that meet the requirements of scientific research. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a method for improving the smoothness of a small table of a SiC anvil for high pressure by polishing. The present invention can greatly improve the polishing of the SiC anvil, meet the requirements of scientific research through traditional mechanical polishing, and improve the production and delivery yield.

[0005] The present invention is realized by the following technical scheme: a method for polishing and improving the surface finish of a small table of a SiC anvil for high pressure, the method comprising the following steps: Step 1, preparing polishing materials, wherein the polishing materials include diamond powder, aluminum powder and olive oil; Step 2: Mix the diamond powder and olive oil evenly, stir until it becomes viscous, and let it stand for a while; Step 3: Add aluminum powder to the mixture, continue to stir evenly, and let it stand for a while; Step 4: Apply the mixed polishing paste evenly on the cast iron plate, and then use the push plate turning stone arm to evenly distribute the polishing paste on the surface of the cast iron plate; Step 5: Use the polishing paste to polish the small SiC anvil table to improve the smoothness of the table.

[0006] As a preferred technical solution, the mass ratio of the diamond powder, aluminum powder and olive oil is 3:4:1, where the mass of the diamond powder is 3, the mass of the olive oil is 1, and the mass of the aluminum powder is 4.

[0007] As a preferred technical solution, the particle size of the diamond powder is W3.5.

[0008] As a preferred technical solution, the olive oil is edible olive oil.

[0009] As a preferred technical solution, the operation duration of evenly applying the polishing paste to the stone pusher arm in step 4 is 30 minutes to ensure that the polishing paste is evenly distributed.

[0010] As a preferred technical solution, the polishing process includes multiple polishings, and cleaning is performed after each polishing, and polishing paste is re-applied.

[0011] As a preferred technical solution, the polishing paste needs to be left to stand for at least 4 hours before use to ensure that all components are fully mixed.

[0012] As a preferred technical solution, the particle size of the aluminum powder is W1.0.

[0013] As a preferred technical solution, the cast iron disc is preheated before use to improve the polishing effect.

[0014] As a preferred technical solution, the polishing process includes multiple polishings, and cleaning is performed after each polishing, and polishing paste is re-applied.

[0015] The beneficial effects of the present invention are as follows: the key point of the present invention is to use W1 diamond powder and W1 aluminum powder, the ratio of 2:8 is prepared with olive oil, and then applied on the cast iron plate, and after the mold is pushed evenly, a layer of W1 diamond aluminum powder is evenly applied on the plate, and when the corresponding polishing of the sample is performed, a good polishing efficiency can be achieved, the finer the number of diamond powder particles, the more it can avoid the occurrence of edge collapse and cracks during the processing process, and the addition of aluminum powder can play a good role in polishing, thereby improving the efficiency and success rate of mechanical polishing and achieving a good effect; By improving the polishing powder, mechanical polishing can achieve a good polishing effect, avoiding secondary optimization and other subsequent complex work. The samples processed by traditional mechanical polishing have poor smoothness on the top pressure anvil, which will cause poor parallelism and make it difficult to reach the ideal pressure value, which cannot meet the requirements of scientific experiments. Compared with the traditional method, the present invention not only improves the polishing effect, but also reduces the production of defective products and increases the yield rate, which meets the strict requirements of high-pressure physics research on the high finish of the anvil table. In addition, the process of the present invention is simple and easy to operate, does not require complex equipment and technology, is suitable for promotion and application under existing production conditions, and has significant economic and technical advantages. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 This is a polishing effect diagram in the prior art; Figure 2 The new polishing effect of the present invention Figure 1 ; Figure 3 The new polishing effect of the present invention Figure 2 . DETAILED DESCRIPTION

[0018] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.

[0019] Any feature disclosed in this specification (including any additional claims, abstract and drawings), unless otherwise stated, may be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.

[0020] The present invention relates to a method for improving the smoothness of a small table of a SiC anvil for high pressure based on polishing, aiming to solve the problem that the SiC anvil is prone to scratches, black stripes and substandard smoothness during the polishing process in the prior art. In order to better understand the present invention, the following describes in detail each implementation step, specific operating conditions, equipment and materials used, and demonstrates the effectiveness and applicability of the method through practical application examples.

[0021] Step 1. Prepare polishing materials: The key to the present invention lies in the polishing materials used and their ratios. First, diamond powder, aluminum powder and olive oil are prepared as polishing materials. Specifically, the particle size of the diamond powder is W3.5, the particle size of the aluminum powder is W1.0, and the olive oil is commercially available edible olive oil. The ratio of the polishing materials is crucial. It is recommended to use a mass ratio of 3:4:1 for diamond powder, aluminum powder and olive oil. Within this range, the ratio can effectively improve the polishing efficiency and reduce material waste. If it is necessary to adjust the polishing effect or adapt to different experimental requirements, the proportion of each component can be appropriately adjusted. For example, the proportion of diamond powder can be increased to further improve the polishing accuracy.

[0022] Step 2: Mix the polishing paste: After preparing the polishing materials, first mix the diamond powder and olive oil. The specific steps are: take 3 mass diamond powder (W3.5), add 1 mass olive oil, and stir the two thoroughly until a viscous paste is formed. When stirring, make sure that the diamond powder and olive oil are evenly mixed to avoid uneven polishing. After stirring, let the mixture stand for 3 hours to allow the components to fully blend. This process ensures that the polishing paste maintains a stable polishing effect in subsequent use.

[0023] Next, add 4 grams of aluminum powder (W1.0), stir again, and let it stand for 1 hour. The addition of aluminum powder can significantly improve the polishing effect and help improve the flatness and finish of the SiC anvil surface. The choice of standing time depends on the uniformity of the mixture to ensure that all ingredients are fully integrated to achieve the best polishing effect.

[0024] Step 3: Prepare the cast iron grinding disc: The cast iron grinding wheel is the main tool for the polishing operation of the present invention. Before polishing, it is recommended to preheat the cast iron grinding wheel. The preheating temperature is usually controlled between 40-60 degrees Celsius. This preheating step helps to reduce the thermal expansion difference of the material during the polishing process and ensure the uniformity and smoothness of the polished surface. The surface of the preheated cast iron grinding wheel needs to be kept clean and flat to avoid any impurities or unevenness that affect the polishing effect.

[0025] Step 4: Apply polishing paste: Apply the mixed polishing paste evenly on the surface of the preheated cast iron grinding disc. During operation, use the pusher stone arm to push back and forth to make the polishing paste evenly cover the entire surface of the grinding disc. To ensure the uniform distribution of the polishing paste, the pushing operation should last at least 30 minutes. If the polishing area is large, the time can be appropriately extended to ensure that all areas to be polished are evenly exposed to the polishing paste. The uniformity of this step is crucial to the final polishing effect.

[0026] Step 5: Polishing SiC anvils: Place the small SiC anvil table to be treated on a cast iron grinding disc coated with polishing paste. During the polishing operation, ensure that the contact surface between the anvil and the grinding disc is always flat, and apply moderate pressure. The polishing movement is usually rotational or reciprocating, and the polishing direction is constantly changed to ensure the uniformity and smoothness of the anvil surface. According to actual needs, the polishing time can be adjusted between 30 minutes and 2 hours to ensure that the polishing effect meets the experimental requirements.

[0027] During the polishing process, be sure to monitor the state of the SiC anvil surface. If necessary, pause the polishing and check the surface quality to avoid over-polishing and material damage. During the inspection process, if it is found that the finish is not up to standard or there are still scratches and streaks on the surface, a second polishing can be performed until the ideal effect is achieved.

[0028] Step 6: Cleaning and Inspection: After polishing, remove the SiC anvil from the grinding disc and clean it thoroughly to remove the polishing paste and other impurities remaining on the surface. Anhydrous ethanol or other suitable cleaning agents can be used during the cleaning process to ensure that there is no residue on the anvil surface. After cleaning, use a microscope to inspect the anvil surface, focusing on the finish, flatness, and the presence of scratches or black streaks.

[0029] If the surface is found to be substandard during testing, it can be decided whether to re-polish or adjust the polishing parameters according to the situation. After multiple polishing, a high-finish SiC anvil that meets the experimental requirements can usually be obtained.

[0030] Example: In order to verify the effectiveness of the method of the present invention, a SiC anvil in a laboratory was selected for treatment. Polishing was performed according to the above steps. After about 1 hour of polishing, the surface of the anvil was detected using a microscope. The results showed that the surface finish of the polished SiC anvil was significantly improved, with no obvious scratches and stripes, meeting the finish requirements of the anvil for high-pressure physics experiments, such as Figure 2 and Figure 3 Compared with the traditional polishing method, the method of the present invention not only excels in improving the finish, but also reduces the polishing time and material loss. Preferred embodiments.

[0031] In some cases, to further improve the polishing effect, finer diamond powder (such as W2.5) can be used or the resting time (such as more than 4 hours) can be extended to ensure that the composition of the polishing paste is more uniform. In addition, during the polishing process, automatic polishing equipment can be used to replace manual operation, thereby further improving the stability and consistency of polishing.

[0032] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that are not conceived through creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.

Claims

1. A method for improving the surface finish of a small table of a SiC anvil for high pressure polishing, characterized in that: The method comprises the following steps: Step 1, preparing polishing materials, wherein the polishing materials include diamond powder, aluminum powder and olive oil; Step 2: Mix the diamond powder and olive oil evenly, stir until it becomes viscous, and let it stand for a while; Step 3: Add aluminum powder to the mixture, continue to stir evenly, and let it stand for a while; Step 4: Apply the mixed polishing paste evenly on the cast iron plate, and then use the push plate turning stone arm to evenly distribute the polishing paste on the surface of the cast iron plate; Step 5: Use the polishing paste to polish the small SiC anvil table to improve the smoothness of the table.

2. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The mass ratio of the diamond powder, aluminum powder and olive oil is 3:4:1, where the mass of the diamond powder is 3, the mass of the olive oil is 1, and the mass of the aluminum powder is 4.

3. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The particle size of the diamond powder is W3.

5.

4. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The olive oil is edible olive oil.

5. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The operation duration of evenly applying the polishing paste to the stone pusher arm in step 4 is 30 minutes to ensure that the polishing paste is evenly distributed.

6. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The polishing process includes multiple polishings, and cleaning is performed after each polishing, and polishing paste is re-applied.

7. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The polishing paste needs to be left to stand for at least 4 hours before use to ensure that the ingredients are fully mixed.

8. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The particle size of the aluminum powder is W1.

0.

9. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The cast iron disc is preheated before use to improve the polishing effect.

10. The method for improving the surface finish of a small table of a SiC anvil for high pressure based on polishing according to claim 1, characterized in that: The polishing process includes multiple polishings, and cleaning is performed after each polishing, and polishing paste is re-applied.

Citation Information

Patent Citations

  • Grinding and polishing paste for high-purity aluminum oxide ceramics

    CN104650741A

  • Diamond paste as well as preparation method and application thereof

    CN106634836A

  • Abrasive and preparation method thereof

    CN107189759A

  • Polishing instrument for dentistry as well as procedure for its manufacturing

    EP0432523A1

  • Grinding and polishing tools

    GB1441899A