Method for manufacturing integrated molded body

By using a mold to clamp and compress the expanded particle molded body, and using steam to form an integrated expanded particle molded body, the problem of poor appearance caused by complex molds and particle mixing in the existing technology is solved, and lightweight and Balance of mechanical strength.

CN118789745AInactive Publication Date: 2024-10-18JIE SI BI SU LIAO DONG GUAN YOU XIAN GONG SI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310390300.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for manufacturing integrated molded bodies require complex molds or mixing different types of foamed particles, resulting in poor appearance.

Method used

A mold consisting of a first mold and a second mold is used to clamp and compress the first expanded particle molded body precursor, fill the second expanded particles, and introduce steam to form the first and second foams. The foam particle molded body is then integrated through welding to achieve the production of an integrated molded body with good appearance.

Benefits of technology

A one-piece molded body with good appearance can be produced without complex molds, ensuring both boundary surface uniformity and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004181684360000191
    Figure BDA0004181684360000191
  • Figure BDA0004181684360000201
    Figure BDA0004181684360000201
  • Figure BDA0004181684360000211
    Figure BDA0004181684360000211
Patent Text Reader

Abstract

The present invention provides a method for manufacturing an integrally molded body capable of manufacturing an integrally molded body having a good appearance without using a complicated device. A method for manufacturing an integrally molded body using a molding die comprising a first molding die and a second molding die, the method comprising: preparing a first foamed particle molded body precursor; the first foamed particle molded body precursor is disposed in a compressed state in the molding die by sandwiching the first foamed particle molded body precursor between the first molding die and the second molding die, the second foamed particles are filled into the molding die, vapor is introduced into the molding die, and the first foamed particle molded body precursor is compressed by the second molding die. A first foamed particle molded body is formed by molding the first foamed particle molded body precursor, a second foamed particle molded body is formed by molding the second foamed particles, and an integrated molded body is obtained by integrating the first foamed particle molded body and the second foamed particle molded body by welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an integrally formed body. Background Art

[0002] The integral molded body obtained by laminating and integrating a plurality of expanded bead molded bodies can change the properties or combination of the expanded bead molded bodies constituting the integral molded body according to the application, and is therefore useful in various fields.

[0003] For example, as disclosed in Patent Documents 1 to 3, various molding devices and manufacturing methods have been proposed as manufacturing devices for the integrally molded body.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Utility Model Publication No. 62-22352

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 54-60366

[0008] Patent Document 3: Japanese Patent Application Publication No. 2009-119748 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] However, the manufacturing apparatuses or methods of the integrally molded bodies described in Patent Documents 1 to 3 have technical problems in that a complicated mold is required or different types of foamed particles are sometimes mixed together, making it impossible to obtain an integrally molded body with a good appearance.

[0011] An object of the present invention is to provide a method for producing an integrally molded body that can produce an integrally molded body having a good appearance without using complicated mold equipment or the like.

[0012] Solutions for solving the above technical problems

[0013] The present inventors have found that the above-mentioned technical problems can be solved by adopting the following configuration.

[0014] That is, the present invention is as follows.

[0015] <1> A method for manufacturing an integral molded body, which is a method for manufacturing an integral molded body using a molding die composed of a first molding die and a second molding die, preparing a first foamed particle molded body precursor, clamping the first foamed particle molded body precursor using the first molding die and the second molding die and arranging the first foamed particle molded body precursor in a compressed state in the molding die, filling the molding die with second foamed particles, introducing steam into the molding die, forming a first foamed particle molded body by molding the first foamed particle molded body precursor, forming a second foamed particle molded body by molding the second foamed particles, and obtaining an integral molded body by integrating the first foamed particle molded body with the second foamed particle molded body by welding.

[0016] <2> The method for producing an integrally molded body according to <1>, wherein the void ratio of the first expanded bead molded body precursor before being arranged in the molding die is 5 to 40%.

[0017] <3> The method for producing an integrally molded article according to <1> or <2>, wherein a density A of the first expanded bead molded article is different from a density B of the second expanded bead molded article.

[0018] <4> The method for producing an integrally molded body according to any one of <1> to <3>, wherein the first expanded bead molded body precursor is clamped and compressed by the first molding die and shrunk to a compression rate of 1 to 20%.

[0019] <5> The method for producing an integrally molded body according to any one of <1> to <4>, wherein the moisture content of the first expanded bead molded body precursor before being arranged in the molding die is 5 to 50% by mass.

[0020] <6> The method for producing an integrally molded body according to any one of <3> to <5>, wherein an absolute value of a difference between a density A of the first expanded bead molded body and a density B of the second expanded bead molded body is 10 to 50 g / L.

[0021] <7> The method for producing an integrally molded body according to any one of <1> to <6>, wherein the first expanded bead molded body precursor is a fused precursor in which first expanded particles are fused to each other by point bonding and have spaces between the first expanded particles.

[0022] <8> The method for producing an integrally molded article according to any one of <1> to <7>, wherein the first expanded bead molded article is a polyolefin resin expanded bead molded article, and the second expanded bead molded article is a polyolefin resin expanded bead molded article.

[0023] <9> A method for manufacturing an integrally formed body as described in any one of <1> to <8>, wherein the first foamed particle constituting the first foamed particle precursor is a multilayer foamed particle consisting of a core layer and a covering layer composed of a resin different from the core layer, and is a multilayer foamed particle capable of being molded at a vapor pressure lower than the molding vapor pressure of a single-layer foamed particle composed of the resin constituting the core layer.

[0024] Effects of the Invention

[0025] According to the present invention, it is possible to provide a method for manufacturing an integrally molded body capable of manufacturing an integrally molded body having a good appearance without using a complicated device. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram illustrating a state where the first expanded bead molded body precursor is arranged in a molding die.

[0027] Figure 2 This is a schematic diagram illustrating a state in which a first expanded bead molded body precursor is in contact with a first molding die and a second molding die constituting a molding die.

[0028] Figure 3 This is a schematic diagram illustrating a state in which a first expanded bead molded body precursor is sandwiched and compressed by a first molding die and a second molding die.

[0029] Figure 4 This is a schematic diagram illustrating a state in which the second expanded beads are filled into a molding die in which the first expanded bead molded body precursor is arranged.

[0030] Figure 5 This is a schematic diagram illustrating a state in which a first expanded bead molded body and a second expanded bead molded body are fused and integrated to form an integral molded body. DETAILED DESCRIPTION

[0031] [Method for producing an integrally molded body]

[0032] The manufacturing method of the integral molded body of the present invention (hereinafter also simply referred to as "the manufacturing method of the integral molded body" or "the manufacturing method of the present invention") is a manufacturing method of the integral molded body using a molding die composed of a first molding die and a second molding die, preparing a first foamed particle molded body precursor, clamping the first foamed particle molded body precursor by the first molding die and the second molding die and arranging the first foamed particle molded body precursor in a compressed state in the molding die, filling the second foamed particles into the molding die, introducing steam into the molding die, forming the first foamed particle molded body by molding the first foamed particle molded body precursor, forming the second foamed particle molded body by molding the second foamed particles, and obtaining the integral molded body by welding and integrating the first foamed particle molded body and the second foamed particle molded body. In addition, in this specification, the numerical range represented by "~" means a range including the numerical values ​​recorded before and after "~" as the lower limit and upper limit.

[0033] In the manufacturing method of the integrally formed body of the present invention, a forming mold composed of a first forming mold and a second forming mold can be used. By combining the first forming mold and the second forming mold, a space for forming the integrally formed body, i.e., a forming mold cavity, is formed in the forming mold. The first forming mold and the second forming mold may also be a movable forming mold and a fixed forming mold. For example, the forming mold cavity may be formed by making the first forming mold a concave mold and the second forming mold a convex mold.

[0034] In the manufacturing method of the integral molded body of the present invention, it is preferred that when a first foamed bead molded body precursor having a size (x) larger than a size (a) in the mold clamping direction when the mold is clamped and compressed by the molding mold, the first foamed bead forming the first foamed bead molded body precursor can be prevented from being mixed with the second foamed bead forming the second foamed bead molded body, so that an integral molded body with good appearance can be manufactured. The size (a) in the mold clamping direction when the molding mold is clamped refers to the size in the mold clamping direction when the molding mold cavity formed by the first molding mold and the second molding mold is clamped.

[0035] The integrally formed body of the present invention is formed by welding a first foamed bead molded body and a second foamed bead molded body together, wherein the first foamed bead molded body is formed by secondary foaming of a first foamed bead molded body precursor disposed in a compressed state in a forming mold. In addition, the integrally formed body of the present invention may further be laminated with other layers.

[0036] <First expanded particle molded article>

[0037] The first foamed bead molded body is preferably of a different type from the second foamed bead molded body described later. "Different types" means that the raw materials, colors or additives of the foamed beads are different, the density of the foamed beads or the density of the molded body is different, and any one of the porosity or other physical properties of the foamed bead molded body is different.

[0038] Preferably, the density A of the first expanded bead molded body is different from the density B of the second expanded bead molded body. By forming the integral molded body from the first expanded bead molded body and the second expanded bead molded body having different densities, for example, an integral molded body having both lightness and characteristics that cannot be obtained from a single molded body can be formed.

[0039] The density A of the first foamed particle molded body is preferably 20 to 250 g / L, more preferably 23 to 200 g / L, further preferably 25 to 150 g / L, further preferably 28 to 100 g / L, further preferably 29 to 70 g / L, from the viewpoint of easily obtaining an integrally molded body with excellent lightness.

[0040] The density A of the first expanded bead molded body can be calculated by cutting out the first expanded bead molded body from the integral molded body and measuring the mass and volume.

[0041] The first expanded bead molded body is preferably composed of first expanded beads described below, and is produced using a first expanded bead molded body precursor having a size larger than a dimension (a) in a mold clamping direction in a mold for molding the integral molded body.

[0042] <Second expanded bead molded article>

[0043] The second expanded bead molded article is preferably of a different kind from the first expanded bead molded article. "Different kind" means that the raw material or physical properties such as color, density, and porosity are different.

[0044] As described above, the density B of the second expanded bead molded body is preferably different from the density A of the first expanded bead molded body. The integrated molded body is formed by welding the first expanded bead molded body and the second expanded bead molded body having different densities, thereby making it easy to achieve both lightness and excellent mechanical strength.

[0045] The density B of the second foamed particle molding is preferably 10 to 250 g / L, more preferably 15 to 200 g / L, further preferably 20 to 150 g / L, further preferably 23 to 100 g / L, and further preferably 25 to 50 g / L, from the viewpoint of easily obtaining an integral molding having lightness and excellent mechanical strength.

[0046] The density B of the second expanded bead molded body can be determined by cutting out the second expanded bead molded body from the integral molded body, measuring the mass and volume, and calculating the apparent density.

[0047] From the viewpoint of moldability of the integrally molded body, the absolute value |AB| of the difference between the density A of the first expanded bead molded body and the density B of the second expanded bead molded body is preferably 10 to 50 g / L, more preferably 10 to 30 g / L.

[0048] In addition, from the viewpoint of moldability of the integral molded body, the density B of the second expanded bead molded body is preferably smaller than the density A of the first expanded bead molded body. From the above viewpoint, the difference (AB) between the density A of the first expanded bead molded body and the density B of the second expanded bead molded body is preferably 10 to 30 g / L.

[0049] (Preparation of the First Expanded Bead Molded Body Precursor)

[0050] The first expanded bead molded body precursor is formed by molding the first expanded bead described below, preferably by in-mold molding of the first expanded bead. The in-mold molding method can be performed by filling the first expanded bead into a molding mold and heating and molding using a heating medium such as steam.

[0051] Specifically, after the first foamed particles are filled into a separately prepared forming mold, a heating medium such as steam is introduced into the forming mold to heat the foamed particles to make them foamed twice, and the foamed particles are welded to each other, so that a first foamed particle precursor (welded precursor) in which the first foamed particles are welded to each other and a shape of a forming space is obtained. The first foamed particle precursor is welded and integrated with the second foamed particle molded body described later to form an integrated molded body.

[0052] As a method for filling the first foamed particles into the forming mold, a known method can be adopted. The filling of the first foamed particles into the forming mold can be listed as: a crack filling method, in which the mold is opened in advance before the first foamed particles are filled into the mold to expand the forming space, and the foamed particles are compressed by closing the mold after filling (for example, Japanese Patent Publication No. 46-38359); a pressurized filling method, in which the first foamed particles are pre-pressurized with a pressurized gas such as air to increase the pressure in the bubbles of the foamed particles, and the pressure in the foamed particles is adjusted to a pressure 0.01 to 0.3 MPa higher than the atmospheric pressure, and then the foamed particles are filled into the forming mold under atmospheric pressure or reduced pressure (for example, Japanese Patent Publication No. 51-22951). In addition, it is also possible to fill the first foamed particles pressurized to a pressure above the atmospheric pressure in the forming mold by a compression filling method (Japanese Patent Publication No. 4-46217) in which the first foamed particles pressurized to a pressure above the atmospheric pressure are filled into the forming mold by using a compressed gas. In addition, the first foamed particles can be filled by filling the foamed particles with high secondary foaming power obtained under special conditions into the mold cavity of the forming mold under atmospheric pressure or reduced pressure by a normal pressure filling method (Japanese Patent Publication No. 6-49795), or a method combining the above methods (Japanese Patent Publication No. 6-22919). In addition, the first foamed particles can be formed by a pressure forming method (for example, Japanese Patent Publication No. 51-22951) in which a heating medium such as steam is supplied to the mold to heat and fuse the first foamed particles. In addition, as a heating method using steam, etc., heat forming can be performed by a method obtained by appropriately combining heating methods such as heating on one side, heating on the other side, and formal heating using a known method.

[0053] The method is not particularly limited, but the first expanded bead molded body precursor is preferably molded by a molding method in which the first expanded beads described below are filled with the first expanded beads by a crack filling method and steam is supplied into a mold to heat and fuse the first expanded beads.

[0054] The temperature of the steam supplied to the molding die is preferably lower than the melting point of the first foamed particles. Specifically, the steam temperature is preferably (melting point of the resin constituting the first foamed particles - 30) ° C to (melting point of the resin constituting the first foamed particles - 5) ° C, and more preferably (melting point of the resin constituting the first foamed particles - 20) ° C to (melting point of the resin constituting the first foamed particles - 10) ° C. The heating time based on steam is preferably 3 to 15 seconds, and more preferably 5 to 10 seconds.

[0055] After steam heating, the forming mold is water-cooled or allowed to cool. After cooling, the first expanded particle precursor is preferably taken out of the forming mold and naturally dried or cured at high temperature.

[0056] The first expanded bead molded article precursor is further subjected to secondary foaming and molding by steam heating when the second expanded bead is molded in a mold as described later, and finally becomes the first expanded bead molded article.

[0057] (First Expanded Bead Molded Body Precursor)

[0058] The first foamed particle molded body precursor is formed by molding the first foamed particles, and has a dimension (x) larger than the dimension (a) in the mold clamping direction of the mold composed of the first mold and the second mold for molding the integral molded body, that is, the dimension (x) of the mold cavity. With such a structure, the first foamed particles can be prevented from being mixed with the second foamed particles described later, and an integral molded body with a relatively uniform boundary surface and good appearance can be obtained.

[0059] The size (x) of the first foamed particle molding precursor is not particularly limited as long as it is larger than the size (a) in the molding mold in the mold closing direction when the molding mold for molding the integral molding is closed, but is preferably 1.01 to 1.3 times the size (a), more preferably 1.07 to 1.2 times, and further preferably 1.10 to 1.18 times.

[0060] From the perspective of steam heating efficiency during the molding of the second foamed particles, the porosity of the first foamed particle molding precursor before it is arranged in the molding mold, that is, before it is clamped and compressed by the first molding mold and the second molding mold that constitute the molding mold is preferably 5 to 40%, more preferably 7 to 35%, and further preferably 8 to 30%.

[0061] In particular, the first expanded bead molded body precursor is preferably a fused precursor in which the first expanded beads are fused to each other by point bonding and there are gaps between the first expanded beads. If such a fused precursor is used, it will not become an obstacle when the steam flows in the molding die when the second expanded beads are molded in the mold, so it is difficult to cause the phenomenon of local excess steam heating, and it is possible to obtain an integral molded body with a more excellent appearance.

[0062] The void ratio of the first foamed particle molded body precursor before being arranged in the forming mold can be measured as follows. A cubic test piece cut out from the first foamed particle molded body precursor before being arranged in the forming mold, i.e. before compression, is sunk into a graduated cylinder filled with ethanol, and the true volume Vc (L) of the test piece is obtained based on the rising part of the liquid level of ethanol. In addition, the apparent volume Vd (L) is obtained based on the outer dimensions (length × width × height) of the test piece. Based on the obtained true volume Vc and apparent volume Vd, the void ratio of the first foamed particle molded body precursor before being arranged in the forming mold can be obtained based on the following formula.

[0063] Void ratio (%) = [(Vd-Vc) / Vd] × 100

[0064] From the perspective of moldability when molding the second foamed particles, the density of the first foamed particle molding precursor before being arranged in the molding mold is preferably 15 to 200 g / L, more preferably 18 to 150 g / L, further preferably 20 to 100 g / L, further preferably 23 to 70 g / L, and further preferably 25 to 60 g / L.

[0065] The skin layer during molding is removed from the first foamed particle molding body precursor before being arranged in the molding mold, and three test pieces are randomly cut out. The mass and volume of each test piece are measured, and the molding density of the three test pieces is calculated. The arithmetic mean value can be calculated as the density of the first foamed particle molding body precursor before being arranged in the molding mold.

[0066] The moisture content of the first expanded bead molded body precursor before being arranged in the molding die is preferably 5 to 50% by mass, more preferably 10 to 45% by mass, further preferably 15 to 42% by mass, and further preferably 17 to 40% by mass.

[0067] Regarding the moisture content of the first foamed particle molding body precursor before being arranged in the molding die, after measuring the mass (M1[g]) of the first foamed particle molding body precursor before being arranged in the molding die, the mass (M2[g]) of the first foamed particle molding body precursor after drying for 2 hours under the conditions of relative humidity of 50%, 80°C, and 1atm is measured. According to the mass M1 of the first foamed particle molding body precursor before drying and the mass M2 of the first foamed particle molding body precursor after drying, the moisture content of the first foamed particle molding body precursor can be calculated based on the following formula.

[0068] Water content (mass %) = [(M1-M2) / M1] × 100

[0069] The shape of the first foamed bead molded body precursor can be appropriately changed according to the shape or color of the desired integral molded body, and when clamped by the first mold and the second mold, it can contact the first mold and the second mold surface. As a result, as long as the first foamed bead molded body precursor can be compressed to the desired compression ratio, it is not particularly limited. The shape of the first foamed bead molded body precursor can be, for example, a spherical or elliptical shape, a cylindrical shape, a rectangular parallelepiped such as a cube, a quadrangular prism shape, a polygonal prism shape such as a triangular prism shape, a cylindrical shape, a rectangular parallelepiped such as a cube, a quadrangular prism shape, a polygonal prism shape such as a triangular prism shape, and a rib protruding in the mold closing direction of the mold is provided at the portion of the boundary surface with the second foamed bead molded body. In the first foamed bead molded body precursor, if a rib protruding in the mold closing direction of the mold is provided at the portion of the boundary surface with the second foamed bead molded body, the shaping property is excellent even when the first foamed bead that is easy to expand is used.

[0070] In addition, when clamped by the first molding die and the second molding die, the shape and size of the first foamed bead molded body precursor other than the size in the mold-closing direction that contacts the first molding die and the second molding die surface are preferably the same shape as the molding space for shaping into the desired shape of the first foamed bead molded body in the molding die of the one-piece molding body, or smaller than the molding space. This is because when the first foamed bead molded body precursor is arranged in the molding die of the one-piece molding body and the second foamed bead is molded, it is preferred that the molding die of the one-piece molding body is molded by closing the mold.

[0071] 《The First Foaming Particles》

[0072] The first expanded particle constituting the first expanded particle molded body precursor may be a single-layer expanded particle, but from the viewpoint of improving the weldability during in-mold molding and facilitating the control of the void ratio, it is preferably a multilayer expanded particle consisting of a core layer and a coating layer. The coating layer may be present on the entire surface of the multilayer expanded particle or on a portion of the surface. In addition, the first expanded particle may also have through holes.

[0073] The multilayer foamed particles are preferably composed of a core layer and a covering layer formed of a resin different from the core layer, and are preferably moldable at a vapor pressure lower than the molding vapor pressure of single-layer foamed particles composed of a resin forming the core layer.

[0074] When the first expanded particle is a multilayer expanded particle, as the resin constituting the core layer, thermoplastic resins, thermoplastic elastomers, etc. can be listed. As thermoplastic resins, polyester resins such as polystyrene resins, polyethylene resins, polyolefin resins, composite resins of polystyrene resins and polyolefin resins, polybutylene succinate, polyethylene terephthalate, polylactic acid, polylactic acid, polycarbonate resins, polyamide resins, etc. can be listed. As thermoplastic elastomers, olefin thermoplastic elastomers, styrene thermoplastic elastomers, polyurethane thermoplastic elastomers, amide thermoplastic elastomers, ester thermoplastic elastomers, etc. can be listed. These can be used alone or in combination of two or more.

[0075] Among them, from the viewpoint of easily obtaining an expanded bead molded body having an excellent balance among mechanical strength, flexibility, processability, etc., the resin constituting the core layer is preferably one or more selected from the group consisting of polyolefin resins and polyolefin thermoplastic elastomers.

[0076] As the polyolefin resin, polyethylene resin, polypropylene resin, etc. can be cited. Among them, the resin constituting the core layer is preferably a polypropylene resin. In this specification, a polypropylene resin refers to a resin in which the content of the structural unit derived from propylene in the resin is 50% by mass or more. The content of the structural unit derived from propylene in the polypropylene resin is preferably 60% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and further preferably 85% by mass or more.

[0077] As the polypropylene resin constituting the core layer, a propylene homopolymer or a propylene copolymer, a mixture thereof, a mixture of a propylene copolymer and a propylene homopolymer, etc. can be used. As the propylene copolymer, a copolymer of propylene and ethylene and / or an α-olefin having a carbon number of 4 to 20 can be exemplified. As the α-olefin, 1-butene, 1-pentene, 1-hexene, 1-octene, 4-methyl-1-butene, etc. can be exemplified.

[0078] Wherein, the polypropylene resin constituting the core layer is preferably a propylene copolymer containing a component derived from ethylene and / or 1-butene as a copolymerization component. As the propylene copolymer, ethylene-propylene copolymer or ethylene-propylene-butene copolymer etc. can be listed. In addition, the propylene copolymer is more preferably a propylene random copolymer.

[0079] As olefin thermoplastic elastomers, there can be cited mixtures of propylene resins and ethylene rubbers, block copolymers of polyethylene blocks and ethylene / α-olefin copolymer blocks, etc. From the viewpoint of the flexibility and heat resistance of the foamed particle molding, the olefin thermoplastic elastomer is preferably a block copolymer of polyethylene blocks and ethylene / α-olefin copolymer blocks.

[0080] Other additives can be added to the core layer within the scope that does not hinder the purpose and effect of the present invention. As other additives, for example, bubble regulators, flame retardants, flame retardant aids, bubble nucleating agents, plasticizers, antistatic agents, antioxidants, UV protection agents, light stabilizers, conductive fillers, antibacterial agents, lubricants, etc. can be listed. As bubble regulators, inorganic powders such as talc, mica, zinc borate, calcium carbonate, silica, titanium oxide, gypsum, zeolite, borax, aluminum hydroxide, and carbon can be listed; organic powders such as phosphoric acid nucleating agents, phenol nucleating agents, amine nucleating agents, and polyvinyl fluoride resin powders. The content of the above-mentioned additives in the core layer is preferably less than 20% by mass, more preferably less than 10% by mass, and further preferably less than 5% by mass.

[0081] When the expanded beads have a single-layer structure, it is preferable to use a resin constituting the core layer.

[0082] The coating layer is preferably composed of a resin different from the resin constituting the core layer. Examples of the resin constituting the coating layer include the above-mentioned thermoplastic resins, the above-mentioned thermoplastic elastomers, etc. These can be used alone or in combination of two or more.

[0083] In addition, the resin constituting the covering layer is preferably composed of a resin that can be molded at a vapor pressure lower than the molding vapor pressure of the core layer single-layer foamed particles, which is the vapor pressure when the single-layer foamed particles composed of the resin constituting the core layer are molded. If the multi-layer foamed particles are composed of such a resin, it is easier to form a point-bonded structure between the foamed particles in the first foamed particle molded body precursor.

[0084] From the viewpoint of weldability or formability, the resin constituting the coating layer is different from the resin constituting the core layer, but preferably is composed of the same resin. Specifically, when the core layer is a polyolefin resin, the coating layer is preferably a polyolefin resin. Further, the coating layer is preferably a polyethylene resin or a polypropylene resin.

[0085] Furthermore, when the core layer and the cladding layer are made of the same resin, for example, it is preferable to use resins having different melting points.

[0086] When the resin constituting the core layer is a polyolefin resin and the resin constituting the covering layer is a polyolefin resin, it is preferred to use a resin having a difference [(A)-(B)] of 1 to 50° C. between the melting point (A) of the polyolefin resin constituting the core layer and the melting point (B) of the polyolefin resin constituting the covering layer, and the difference is more preferably 3 to 30° C., and further preferably 5 to 20° C. As described above, it is easier to make the resin constituting the covering layer consist of a resin that can be molded at a lower vapor pressure than the molding vapor pressure of the core layer single-layer foamed particles, which is the vapor pressure when the single-layer foamed particles composed of the resin constituting the core layer are molded.

[0087] In the range that does not hinder the purpose effect of the present invention, other additives can be added to the coating layer. The examples of other additives are the same as other additives that can be added to the core layer. The content of the above-mentioned additives in the coating layer is preferably below 20 mass %, more preferably below 10 mass %, and further preferably below 5 mass %.

[0088] When the first foamed particle is a multilayer foamed particle, the mass ratio of the coating layer to the core layer is preferably 1:99 to 20:80. If the mass ratio of the coating layer to the core layer is within the above range, the weldability is more excellent and the secondary foaming during in-mold molding can be more reliably suppressed. Based on the above viewpoint, the mass ratio of the coating layer to the core layer is more preferably 2:98 to 15:85, and further preferably 5:95 to 10:90.

[0089] The method for producing multilayer expanded particles is not particularly limited, and examples thereof include a method of foaming multilayer resin particles having a core layer and a coating layer, or a method of attaching a coating layer to a foamed particle precursor after obtaining a foamed particle precursor to produce multilayer expanded particles. In the case of foaming multilayer resin particles having a core layer and a coating layer to obtain first expanded particles, when granulating the resin particles, it is preferred to laminate the coating layer onto the surface of the core layer by coextrusion.

[0090] From the viewpoint of giving a good appearance to the molded body, the first expanded particle may further contain a pigment. The pigment may be any of an inorganic pigment and an organic pigment, but is preferably an inorganic pigment. When the expanded particle is made into a colored material, the pigment may be added to the core layer and / or the coating layer.

[0091] Examples of the inorganic pigment include black inorganic substances such as carbon black, carbon nanotubes, graphene, iron black, and titanium black; white inorganic substances such as titanium dioxide, zinc oxide, silicon dioxide, aluminum oxide, magnesium oxide, antimony trioxide, barium sulfate, and lithopone; red inorganic substances such as red iron oxide; yellow inorganic substances such as iron yellow and zinc yellow; green inorganic substances such as chrome green and cobalt green; and blue inorganic substances such as ultramarine blue, Prussian blue, cobalt blue, and YInMn (yttrium indium manganese) blue.

[0092] From the viewpoint of being able to impart a good black appearance, the inorganic pigment preferably contains carbon black and / or titanium oxide. In addition, when the inorganic pigment contains carbon black, the proportion of carbon black in the inorganic pigment is preferably 50% by mass or more, more preferably 60% by mass or more, further preferably 80% by mass or more, and further preferably 90% by mass or more.

[0093] As carbon black, for example, channel black, roll black, furnace black, thermal black, acetylene black and the like can be used.

[0094] When the first foamed particles contain inorganic pigments, the content of the inorganic pigments in the first foamed particles is preferably 0.01 to 10% by mass, more preferably 0.05 to 8% by mass, further preferably 0.1 to 5% by mass, and further preferably 2 to 4% by mass, from the viewpoint of suppressing the occurrence of color unevenness in the integrally formed body, easily obtaining an integrally formed body with a good appearance, and stably obtaining the first foamed particles with good in-mold formability.

[0095] For example, the first expanded particles can be produced by releasing resin particles containing a foaming agent dispersed in an aqueous medium in a closed container together with the aqueous medium from the container into a pressure atmosphere lower than the pressure in the container to foam the resin particles.

[0096] The first expanded particles obtained as described above can be pressurized with air or the like to increase the pressure (internal pressure) in the bubbles of the expanded particles, and then heated with steam or the like to expand them (two-stage expansion), thereby producing expanded particles with a higher expansion ratio (lower bulk density).

[0097] 《Second foaming particles》

[0098] As the resin constituting the second foamed particles, the resins exemplified as the resin constituting the first foamed particles can be used. Therefore, it is preferred that the first foamed particle molded body composed of the first foamed particles is a polyolefin resin foamed particle molded body, and the second foamed particle molded body composed of the second foamed particles is a polyolefin resin foamed particle molded body.

[0099] The second foamed particle may be a single-layer foamed particle, or from the viewpoint of improving the weldability during in-mold forming, may be a multi-layer foamed particle consisting of a core layer and a coating layer. When the second foamed particle is a multi-layer foamed particle, the coating layer may be present on the entire surface of the multi-layer foamed particle, or may be present on a portion of the surface. In addition, the second foamed particle may also have through holes.

[0100] A preferred method for producing the second expanded particles is also the same as the preferred method for producing the first expanded particles.

[0101] The second foamed particle molded body is preferably different in density from the first foamed particle molded body. At the stage of the foamed particles, the density of the first foamed particles and the density of the second foamed particles may also be different. In addition, the first foamed particles and the second foamed particles may also be different because either one of the first foamed particles and the second foamed particles contains a pigment, and either one of the first foamed particles and the second foamed particles does not contain a pigment, or the content of the pigment is different. In addition, the content of the pigment of the first foamed particle and the second foamed particle may also be different, and the type of the pigment used by the first foamed particle and the second foamed particle may also be different. In the case where the two are different, a heterogeneous molded body can be obtained as the foamed particle molded body.

[0102] Hereinafter, preferred embodiments for implementing the present invention will be described using the drawings. In addition, the following embodiments do not limit the invention of each claim, and all combinations of features described in the embodiments are not necessarily essential to the solution of the invention.

[0103] (Arrangement of the First Foamed Bead Molded Body Precursor 21 in the Molding Mold 10)

[0104] like Figure 1As shown, the first foamed particle molded body precursor 21 is arranged in the molding die 10 composed of the first molding die 11 and the second molding die 12. In the case where the first molding die 11 and the second molding die 12 constituting the molding die 10 are a movable molding die and a fixed molding die, the first foamed particle molded body precursor 21 can be arranged at a desired position of the fixed molding die. In addition, the first molding die 11 and the second molding die 12 can also be movable molding die. In the case where the first molding die 11 and the second molding die 12 are both movable molding die, there is no particular limitation, and the first foamed particle molded body precursor 21 can be arranged on the side with less movement in the mold closing direction described later. In addition, in Figure 1 In the embodiment, the first forming die 11 is a concave die, and the second forming die 12 is a convex die, thereby forming a pair of forming dies.

[0105] The molding die 10 may include a holding member 15 for holding the first foamed particle molded body precursor 21. The holding member 15 may be configured in a manner that surrounds the outer periphery of the first foamed particle molded body precursor 21 and embeds the first foamed particle molded body precursor 21, or may be a plate-like member disposed on the vertical side of the first foamed particle molded body precursor 21 to limit the displacement of the first foamed particle molded body precursor 21 in the vertical direction for holding. In addition, the holding member 15 may also be discontinuous. That is, the holding member 15 may be configured in a manner that a plurality of plate-like members surround the outer periphery of the first foamed particle molded body precursor 21, or may be configured in a manner that a plate-like member disposed on the vertical side of the first foamed particle molded body precursor 21 is composed of a plurality of plate-like members. In the case where the holding member 15 of the first foamed particle molded body precursor 21 is composed of a plurality of plate-like members, the intervals thereof may be equal intervals or may not be equal intervals.

[0106] Furthermore, the holding member 15 of the first expanded bead molded body precursor 21 may be a member that pierces the first expanded bead molded body precursor 21 to fix the first expanded bead molded body precursor 21 .

[0107] Although not particularly limited, Figure 1 to Figure 5 As shown, when the first foamed particle molded body precursor 21 is arranged in the second molding die 12, the first molding die 11 without the first foamed particle molded body precursor 21 can be provided with a second foamed particle filler 17 (see Figure 4 ).

[0108] (Clamping and Compression of the First Foamed Bead Molded Body Precursor 21 by the Molding Die 10)

[0109] like Figure 1As shown, after the first foamed particle molded body precursor 21 is arranged in the molding die 10, for example, the second molding die 12, at least one of the first molding die 11 and the second molding die 12 is moved to the Figure 1 The two arrows show the direction of mold closing, so that Figure 2 As shown, the first foamed particle molded body precursor 21 is in contact with the first molding die 11 and the second molding die 12. By further moving at least one of the first molding die 11 and the second molding die 12 toward Figure 1 The two arrows show the direction of mold closing, so that Figure 3 As shown, the first foamed bead molded body precursor 21 is clamped and compressed by the first mold 11 and the second mold 12 constituting the mold 10. The first foamed bead molded body precursor 21 has a relatively Figure 3 The dimension (a) in the mold clamping direction of the mold 10 when the mold 10 is clamped is larger than the dimension (x) (see Figure 1 and Figure 2 ), before the first molding die 11 and the second molding die 12 constituting the molding die 10 are molded together, the first foamed bead molding body precursor 21 is in contact with the first molding die 11 and the second molding die 12. Then, when the first molding die 11 and the second molding die 12 constituting the molding die 10 are molded together, the first foamed bead molding body precursor 21 is arranged in the molding die 10 in a state of being clamped and compressed by the first molding die 11 and the second molding die 12.

[0110] The compression rate of the first foamed bead molded body precursor 21 when it is compressed by being clamped by the first molding die 11 and the second molding die 12 constituting the molding die is preferably 1 to 20%. If the compression rate is within the above range, it is possible to more effectively prevent the first foamed bead (not shown, the same below) forming the first foamed bead molded body precursor 21 from being mixed with the second foamed bead E2 forming the second foamed bead molded body 32, and it is easy to obtain an integral molded body 100 having a desired boundary surface and good appearance (see Figure 4 and Figure 5 More specifically, if the second foamed particle E2 is molded at the above compression ratio, the second foamed particle E2 can be filled in the mold 10 of the integral molded body 100 while the first foamed particle molded body precursor 21 is in contact with the first mold 11 and the second mold 12 (see Figure 4 Therefore, the second expanded particle E2 does not enter between the molding die 10 and the first expanded particle molded body precursor 21 (refer to Figure 4 ). After that, since the second foamed particle E2 is formed, the boundary surface between the first foamed particle molded body 31 and the second foamed particle molded body 32 can be formed in a uniform state (refer to Figure 4 and Figure 5 ).

[0111] The compression rate can be calculated based on the following formula.

[0112] Compression rate (%) = [(dimension of the first foamed bead molded body precursor 21 in the mold clamping direction after compression (dimension in the mold clamping direction when the mold 10 is clamped (a))) / (dimension of the first foamed bead molded body precursor 21 in the mold clamping direction before compression)] × 100

[0113] When the shape of the integrally molded body is complicated, the size of the portion with the highest compression rate obtained by the above formula is adopted.

[0114] (Filling of Second Expanded Particles E2)

[0115] like Figure 4 As shown, the second foamed particle E2 forming the second foamed particle molded body 32 is filled into the mold 10 provided with the first foamed particle molded body precursor 21 clamped and compressed by the first mold 11 and the second mold 12. As the filling method of the second foamed particle E2, the above-mentioned crack filling method, pressure filling method, etc. can be listed, but the crack filling method is preferred. Figure 4 Although one second expanded particle E2 filled in the forming mold 10 is shown in FIG. 1 , a plurality of second expanded particles E2 are filled in the forming mold 10 .

[0116] (Formation of Integrally Molded Body 100)

[0117] After the second expanded particles E2 forming the second expanded particle molded body 32 are filled into the molding die 10, steam is introduced into the molding die 10 filled with the second expanded particles E2 (see Figure 4 ). In the molding die 10 of the integral molding body 100, the second foamed particles E2 are foamed twice, and the second foamed particles E2 are fused to each other to form a second foamed particle molded body 32, and the first foamed particle molded body precursor 21 is foamed twice to form a first foamed particle molded body 31 formed by foaming the first foamed particle molded body precursor, as shown in FIG. Figure 5 As shown, the integrated molded body 100 in which the first foamed bead molded body 31 and the second foamed bead molded body 32 are welded and integrated can be obtained. That is, by welding the first foamed particles forming the first foamed bead molded body 31 and the second foamed bead molded body 32, and welding the first foamed bead molded body 31 and the second foamed bead molded body 32, the integrated molded body 100 in which the first foamed bead molded body 31 and the second foamed bead molded body 32 are integrated can be obtained. As a heating method using steam or the like, the integrated molded body 100 can be formed by heating and molding by a method in which a heating method such as heating on one side, heating on the other side, and regular heating are appropriately combined using a known method.

[0118] The temperature of the steam supplied to the molding die 10 is preferably lower than the melting point of the second foamed particle E2. Specifically, the steam temperature is preferably (melting point of the resin constituting the second foamed particle E2 - 30) ° C to (melting point of the resin constituting the second foamed particle E2 - 5) ° C, and more preferably (melting point of the resin constituting the second foamed particle E2 - 20) ° C to (melting point of the resin constituting the second foamed particle E2 - 10) ° C. By heating to the above temperature, the particles of the second foamed particle E2 are fused to each other, and the first foamed particle and the second foamed particle E2 can be fused at the surface in contact with the first foamed particle.

[0119] From the viewpoint of easily obtaining an integrally formed body 100 having a good and smooth appearance, the heating time with steam is preferably 10 to 60 seconds, more preferably 20 to 50 seconds.

[0120] After steam heating, the mold 10 is water-cooled and left to cool. The cooling time is adjusted so that the secondary foaming force of the integral molded body 100 is reduced and so that the integral molded body 100 does not expand or shrink after demolding.

[0121] After cooling, the integral molded body 100 is taken out from the mold 10. In order to further suppress shrinkage, the integral molded body 100 taken out from the mold 10 is preferably subjected to high temperature curing. The high temperature curing is preferably placed in an atmosphere of 60 to 80° C. for more than 4 hours, and after a predetermined time, the temperature is gradually lowered until it becomes 40° C. or less.

[0122] The integral molded body 100 obtained by the manufacturing method of the integral molded body of the present invention can change the physical properties such as raw materials or color, density, and porosity in the first foamed particle molded body 31 part and the second foamed particle molded body 32 part. In addition, since the second foamed particle E2 is prevented from accidentally mixing into the first foamed particle molded body 31 part, there is a desired uniform boundary surface between the first foamed particle molded body 31 and the second foamed particle molded body 32, and the appearance is excellent. For example, by configuring the first foamed particle molded body 31 with a higher density in the part where strength is required, and configuring the second foamed particle molded body 32 with a lower density in the other part, it is easy to obtain an integral molded body 100 with excellent lightness and mechanical strength. In addition, by changing the color of the first foamed particle molded body 31 and the color of the second foamed particle molded body 32, it is easy to obtain an integral molded body 100 with excellent design.

[0123] [Example]

[0124] Next, the present invention will be described in further detail using examples, but the present invention is not limited to these examples at all.

[0125] [Measurement and evaluation]

[0126] The following measurements and evaluations were performed on the expanded particles, the first expanded particle molded body precursor, the expanded particle molded body (the first expanded particle molded body and the second expanded particle molded body), and the integral molded body used in the examples. In addition, the measurements and evaluations on the expanded particles, the first expanded particle molded body precursor, the expanded particle molded body, and the integral molded body were performed after they were placed for 2 days under the conditions of a relative humidity of 50%, 23°C, and 1 atm for conditioning. In addition, the measurements on the first expanded particle molded body precursor were performed on the precursor before being arranged in the molding mold.

[0127] <Foamed particles>

[0128] (Volume Density)

[0129] About 500cm 3 Fill the expanded particle group into the measuring cylinder, and tap the bottom of the measuring cylinder on the ground several times to stabilize the filling height of the expanded particle group in the measuring cylinder. Read the gross volume of the expanded particle group indicated by the measuring cylinder scale and set it as V1 (L). Next, measure the mass of the expanded particle group and set it as W1 (g).

[0130] The weight W1[g] of the foamed particles is divided by the volume V1 to calculate (W1 / V1), and the unit is converted to [kg / m 3 ], and the volume density of the foamed particles is calculated.

[0131] <First expanded bead molded article precursor>

[0132] (Porosity)

[0133] The porosity of the first foamed particle molded body precursor was measured as described below. A cubic test piece cut out from the first foamed particle molded body precursor was sunk into a graduated cylinder filled with ethanol, and the true volume Vc (L) of the test piece was calculated based on the rising portion of the liquid level of ethanol. In addition, the apparent volume Vd (L) was calculated based on the outer dimensions (length × width × height) of the test piece. Based on the calculated true volume Vc and apparent volume Vd, the porosity of the first foamed particle molded body precursor was calculated based on the following formula.

[0134] Void ratio (%) = [(Vd-Vc) / Vd] × 100

[0135] (Water content)

[0136] Regarding the moisture content of the first foamed particle molding precursor, after measuring the mass (M1[g]) of the first foamed particle molding precursor, the mass (M2[g]) of the first foamed particle molding precursor after drying for 2 hours under the conditions of relative humidity of 50%, 80°C, and 1atm is measured. From the mass M1 of the first foamed particle molding precursor before drying and the mass M2 of the first foamed particle molding precursor after drying, the moisture content of the first foamed particle molding precursor is calculated based on the following formula.

[0137] Water content (mass %) = [(M1-M2) / M1] × 100

[0138] <First Expanded Bead Molded Article Precursor and Expanded Bead Molded Article>

[0139] (density)

[0140] The epidermal layer during molding is removed from the first foamed particle molding precursor or the integral molding, and three test pieces are randomly cut out so as to form a rectangular shape of 50 mm long × 50 mm wide × 25 mm thick. The mass and volume of each test piece are measured, and the apparent density of the three test pieces is calculated. The arithmetic mean value is obtained as the density of the first foamed particle molding precursor and the foamed particle molding.

[0141] <One-piece molded body>

[0142] (Appearance)

[0143] The appearance of the integrally molded body was evaluated according to the following criteria.

[0144] A: The boundary surface between the first expanded bead molded body and the second expanded bead molded body is formed uniformly.

[0145] B: At the boundary between the first expanded bead molded body and the second expanded bead molded body, the expanded beads of one enter the molded body side of the other, and a partially mixed expanded bead molded body is formed.

[0146] (shrink)

[0147] Evaluation regarding die surface following of the integral molded body was performed according to the following criteria.

[0148] A: The error with the forming die is within 10% and an integrally formed body is formed.

[0149] B: After forming, some local shrinkage is visible, but the average error with the forming die is within 10%.

[0150] C: After molding, significant shrinkage was observed, and an integral molded body of the target size could not be obtained.

[0151] [raw material]

[0152] The raw materials used in Examples and Comparative Examples are shown below.

[0153] <Resin>

[0154] ·R1: Polypropylene resin (melting point 141°C, tensile modulus 930 MPa, MFR 8 g / 10 min)

[0155] ·R2: Polypropylene resin (melting point 128°C, tensile modulus 650MPa, MFR 7g / 10min)

[0156] ·R3: Polypropylene resin (melting point 146°C, tensile modulus 950 MPa, MFR 9 g / 10 min)

[0157] ·R4: Polypropylene resin (melting point 132°C, tensile modulus 830 MPa, MFR 7 g / 10 min)

[0158] The melting points of the various polypropylene resins are determined based on JIS K7121:1987. Specifically, a test piece composed of polypropylene resin foam particles is first prepared, and the state of the test piece is adjusted based on "(2) After a certain heat treatment, the melting temperature is measured" in JIS K7121:1987. The heating rate and cooling rate in the state adjustment are both set to 10°C / min. The DSC curve is obtained by heating the state-adjusted test piece from 30°C to 200°C at a heating rate of 10°C / min, and the vertex temperature of the melting peak appearing in the DSC curve is set as the melting point Tmc. In addition, when multiple melting peaks appear in the DSC curve, the vertex temperature of the melting peak with the largest area is set as the melting point Tmc.

[0159] The melt flow rates (ie, MFR) of the resins shown above are measured in accordance with JIS K7210-1:2014 under the conditions of a temperature of 230° C. and a load of 2.16 kg.

[0160] The tensile modulus of the polypropylene resin is measured by hot pressing a sample at 230° C. to form a sheet, making a No. 2 test piece with a sample thickness of 1 mm in accordance with JIS K6758, at a test speed of 0.25 mm / min.

[0161] [Manufacturing of expanded particles]

[0162] Production Examples 1, 2 and 4

[0163] A device in which a multilayer wire harness forming die is installed on the outlet side of an extruder for a resin particle core layer with an inner diameter of 50 mm and an extruder for a resin particle welding layer with an inner diameter of 30 mm is used. The resin shown in Table 1 is supplied to the extruder for forming the core layer, and melt-kneaded to form a core layer forming melt kneaded product, and the resin shown in Table 1 is supplied to the extruder for forming the coating layer, and melt-kneaded to form a coating layer melt kneaded product. Next, the core layer forming melt kneaded product and the coating layer forming melt kneaded product are introduced into the multilayer wire harness forming die and merged, and extruded from the small hole of the die installed at the front end of the extruder in a wire harness shape (core layer: 95% by mass, coating layer: 5% by mass), after water cooling, cut and dried in a granulator with a mass of 1.2 mg and an aspect ratio (L / D) of 3, thereby obtaining multilayer resin particles. In addition, zinc borate as a bubble regulator is added to the resin composition constituting the core layer so that its content is 0.1 parts by mass relative to 100 parts by mass of the multilayer resin particles.

[0164] 60L of water as a dispersion medium, 20kg of the obtained multilayer resin particles, 15g of kaolin as a dispersant, and 2.5MPa (G) of carbon dioxide as a foaming agent were pressed into a sealed container with a volume of 100L to obtain foamable multilayer resin particles. Next, the sealed container was opened, and the foamable multilayer resin particles and the dispersion medium were released from the sealed container to atmospheric pressure to obtain foamed particles. The physical properties of the obtained foamed particles are shown in Table 1. In addition, (G) represents the instrument pressure.

[0165] Production example 3

[0166] In Production Example 1, resin particles having a single-layer structure were produced using only the core layer forming extruder. Expanded particles were produced in the same manner as in Production Example 1 except for this.

[0167] [Table 1]

[0168]

[0169] [Manufacturing of Second Expanded Beads]

[0170] Resin particles and expanded particles were prepared in the same manner as above except that carbon black was added to the resin of the core layer to color it black in Preparation Example 1. The bulk density of the second expanded particles was 30 g / L.

[0171] [Manufacturing of the First Expanded Bead Molded Body Precursor]

[0172] Production Examples 1 to 7

[0173] A flat plate-shaped mold of 100 mm in length × 50 mm in width × 58 mm in thickness was moved in a manner to obtain the cracking amount shown in Table 2, filled with the first foamed particles shown in Table 2, and molded by introducing steam (0.2 to 0.3 MPa (G)) into the mold. Specifically, steam was sequentially applied to heat one side of the mold, heat the other side of the mold opposite to the other side of the mold, and heat both sides of the mold from both sides, followed by cooling, and molding under the same conditions to obtain a first foamed particle molded body precursor. The physical properties of the obtained first foamed particle molded body precursor are shown in Table 2.

[0174] [Table 2]

[0175]

[0176] [Manufacturing of integrally molded body]

[0177] Examples 1 to 9, Comparative Examples 1 and 2

[0178] As a mold for an integrally formed body, a mold having a forming cavity of 500 mm long × 200 mm wide × 50 mm thick, which is composed of a first forming mold and a second forming mold, is prepared. In addition, in this mold, the thickness direction is the mold closing direction. The first foamed particle forming body precursor shown in Table 3 is arranged in a forming mold composed of a first forming mold and a second forming mold, and the first foamed particle forming body precursor is clamped and compressed by the first forming mold and the second forming mold to shrink it to a compression ratio shown in Table 3. The amount of cracking at this time is the value shown in Table 3. Next, the second foamed particles shown in Table 3 are filled in the forming mold, and steam (0.2 to 0.3 MPa (G)) is introduced into the forming mold. After heating one side, the other side, and both sides by steam, it is cooled and formed under the same conditions to obtain an integrally formed body. The physical properties of the obtained integrally formed body are shown in Table 3.

[0179] [Table 3]

[0180]

[0181] As can be seen from the results shown in Table 3, the integrally molded bodies of Examples have good appearance and are excellent in mold following.

[0182] Description of Reference Numerals

[0183] 100 one-piece molded body

[0184] 10 Forming die

[0185] 11First forming die

[0186] 12 Second forming die

[0187] 15. Keeping parts

[0188] 17 The second foam particle filler

[0189] 21 first expanded particle molded body precursor

[0190] 31 first expanded particle molded body

[0191] 32 second expanded particle molding

[0192] aThe dimensions of the cavity in the mold closing direction when the forming mold is closed

[0193] x is the dimension in the mold clamping direction of the first expanded bead molded body precursor before being arranged in the molding die.

[0194] E2 second expanded particles.

Claims

1. A method for manufacturing an integrally formed body, comprising: using a forming die composed of a first forming die and a second forming die to manufacture the integrally formed body; It is characterized in that preparing a first expanded particle molded body precursor, The first foamed bead molded body precursor is clamped by the first molding die and the second molding die, and the first foamed bead molded body precursor is arranged in the molding die in a compressed state. Filling the second expanded particles into the forming mold, Steam is introduced into the forming mold, and a first foamed particle molded body is formed by molding the first foamed particle molded body precursor, and a second foamed particle molded body is formed by molding the second foamed particle, and an integral molded body is obtained by welding the first foamed particle molded body and the second foamed particle molded body together.

2. The method for manufacturing an integrally formed body according to claim 1, It is characterized in that The porosity of the first expanded bead molded body precursor before being arranged in the molding die is 5 to 40%.

3. The method for manufacturing an integrally formed body according to claim 1 or 2, It is characterized in that The density A of the first expanded particle molded body is different from the density B of the second expanded particle molded body.

4. The method for manufacturing an integrally formed body according to claim 1 or 2, It is characterized in that The first expanded bead molded body precursor is clamped and compressed by the first molding die and is reduced so that the compression rate becomes 1 to 20%.

5. The method for manufacturing an integrally formed body according to claim 1 or 2, It is characterized in that The moisture content of the first expanded bead molded body precursor before being arranged in the molding die is 5 to 50% by mass.

6. The method for manufacturing an integrally formed body according to claim 3, It is characterized in that The absolute value of the difference between the density A of the first expanded particle molded body and the density B of the second expanded particle molded body is 10 to 50 g / L.

7. The method for manufacturing an integrally formed body according to claim 1 or 2, It is characterized in that The first expanded bead molded body precursor is a fused precursor in which first expanded particles are fused to each other by point bonding and have spaces between the first expanded particles.

8. The method for manufacturing an integrally formed body according to claim 1 or 2, It is characterized in that The first expanded particle molded body is a polyolefin resin expanded particle molded body, and the second expanded particle molded body is a polyolefin resin expanded particle molded body.

9. The method for manufacturing an integrally formed body according to claim 7, It is characterized in that The first foamed particles are multilayer foamed particles composed of a core layer and a covering layer composed of a resin different from the core layer, and are multilayer foamed particles that can be molded at a vapor pressure lower than the molding vapor pressure of single-layer foamed particles composed of a resin constituting the core layer.