Preparation method of hexagonal boron nitride nanosheet
By combining boron powder with pure sodium chloride or sodium chloride as molten salt to synthesize hexagonal boron nitride nanosheets at high temperature under nitrogen conditions, the problems of complex process, high cost and environmental protection in the existing technology are solved, and high-purity nanosheets are achieved The preparation and recovery of molten salt are suitable for large-scale production.
Patent Information
- Application Number
- CN202410786000.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
Smart Images

Figure CN118790959A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for preparing hexagonal boron nitride nanosheets. Background Art
[0002] Hexagonal boron nitride (h-BN), known as "white graphene", is a non-oxide ceramic with a graphite-like structure, which has excellent thermal conductivity, oxidation resistance, insulation performance and low thermal expansion coefficient. h-BN is widely used in the field of thermal interface materials as a thermal conductive filler, especially in the field of electronic industry to form high thermal conductivity and insulation composite materials with polymers. Compared with ordinary boron nitride particles, boron nitride nanosheets (BNNS) have a larger specific surface area and a larger thermal contact area when composited with matrix materials. They can increase the thermal conductivity pathway in the material and improve the thermal conductivity efficiency. At present, the methods of directly synthesizing hexagonal boron nitride nanosheets using "bottom-up" chemical reactions include pulsed plasma deposition, chemical vapor deposition, magnetron sputtering, ion beam, precursor pyrolysis and molten salt-assisted synthesis. Among them, pulsed plasma deposition and chemical vapor deposition can efficiently prepare single-layer or multi-layer hexagonal boron nitride nanosheets with controllable thickness and high purity. They mainly use small molecular gases of boron or nitrogen such as ammonia borane, borazane or diborane as precursors to react on the surface of substrates such as copper, silver, nickel and platinum to generate BNNS. However, the preparation process is complicated and requires specific atmosphere and vacuum or pressure conditions. It has high requirements for equipment and low yield, which is not suitable for large-scale preparation. Magnetron sputtering, ion beam method and precursor pyrolysis method are effective ways to prepare h-BNNS on a large scale, but magnetron sputtering and ion beam method usually require pretreatment of the substrate in a hydrogen, argon or nitrogen atmosphere at a high temperature of about 1000°C, and then sputter the target through an ion beam of a certain intensity, which has high requirements for equipment and complex preparation process. The precursor pyrolysis method is generally divided into two steps: preparation of the precursor and high-temperature cracking. Most precursors are prepared using organic raw materials, which have problems such as long preparation cycle and poor environmental protection of raw materials. In addition, “YeLinfeng, Zhao Lei, Liang Feng, He Xuan, Fang Wei, Chen Hui, Zhang Shaowei, AnShihua. Facile synthesis of hexagonal boron nitride nanoplates via molten-salt-mediated magnesiothermic reduction[J]. Ceramics International, 2015, 41(10): 14941-14948.” reported a preparation method of h-BNNS synthesized by molten salt-assisted magnesiothermic reduction.Sodium tetraborate and magnesium metal powder are used as reaction raw materials, and magnesium chloride is used as an auxiliary molten salt medium. First, sodium tetraborate / magnesium metal is weighed and mixed according to a molar ratio of 1:6, and different proportions of magnesium chloride are added to the mixed raw materials (the mass ratio of magnesium chloride / reactant is 0.5:1, 1:1, 2:1, 4:1), and then placed in an alumina tube furnace and heated to 800-1200°C at 5°C / min under a nitrogen atmosphere for 3 hours and then cooled to room temperature. Finally, it is stirred in sulfuric acid (5wt%) for 12 hours to remove impurities, and then washed with deionized water, filtered, and dried to obtain h-BNNS. In this method, the chemical properties of the reaction raw material magnesium are active, difficult to preserve, and easy to oxidize and spontaneously combust, which is dangerous. In addition, the product impurity removal time is long, and there is a problem of sulfuric acid waste liquid treatment and discharge. "Tian Liang, Li Junyi, Liang Feng. Chang Shuai, Zhang Haijun, Zhang Mingyang, Zhang Shaowei. Facilemolten salt synthesis of atomically thin boron nitride nanosheets and their co-catalytic effect on the performance of carbon nitride photocatalyst [J]. Journal of Colloid and Interface Science, 2019, 536: 664–672." reported a method for molten salt-assisted synthesis of h-BNNS. In this method, melamine is used as a nitrogen source, borax is used as a boron source, and a mixed salt of sodium chloride and potassium chloride is used as an auxiliary molten salt. The mixed raw materials are placed in an alumina crucible and heated to 1100°C at 4°C / min in a nitrogen atmosphere for 3 hours, then cooled to room temperature with the furnace. The initial powder is obtained by washing and drying, and finally h-BNNS is obtained by ultrasound and centrifugation. This method has the characteristics of cheap production equipment, simple process and high product yield, but the raw material melamine used is a Class 2B carcinogen and has certain hazards to both human body and environment.Patent CN1161216661A discloses a preparation method for synthesizing h-BNNS by combining a precursor method with a molten salt-assisted method. The invention uses boric acid, borax and boron oxide as boron sources, melamine, urea, melamine and diamide as nitrogen sources, and mixes and grinds them according to a molar ratio of N and B atoms of 1:1-1:6, and then heats them to 250-300°C in a nitrogen atmosphere for 4-8 hours to generate a precursor. The precursor is then uniformly mixed with one or more molten salts such as sodium chloride, potassium chloride and potassium carbonate at a mass ratio of precursor / molten salt of 1:1-1:4. Finally, the temperature is raised to 1200-1500°C in a nitrogen atmosphere with a gas flow rate of 0.3-0.8L / min, and the mixture is kept for 3-6 hours, then cooled to room temperature with the furnace, and washed and dried to obtain h-BNNS. The use of raw materials such as melamine in this method is not environmentally friendly. Both the precursor preparation and molten salt-assisted sintering require a long time, and there are problems such as long preparation time and complicated process steps.
[0003] Therefore, it is necessary to solve the problems of complex process, high economic cost and environmental protection in the preparation of hexagonal boron nitride nanosheets. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing hexagonal boron nitride nanosheets, which has the characteristics of simple operation, cheap raw materials, non-toxicity, and suitability for large-scale production.
[0005] The preparation method of hexagonal boron nitride nanosheets of the present invention comprises the following steps: mixing boron powder and molten salt, synthesizing them at high temperature under nitrogen conditions, and separating the synthesized products to obtain hexagonal boron nitride nanosheets h-BNNS and recyclable molten salt;
[0006] Further, the mass ratio of the molten salt to the boron powder is 1:1-10:1;
[0007] Further, the molten salt is one of pure sodium chloride and pure potassium chloride or a mixture of the two;
[0008] Further, the boron powder and the molten salt are mixed by mechanical grinding to obtain a mixed powder, and the grinding time is 10-30 minutes;
[0009] Further, the mixed powder is heated to 1000-1400° C. in a nitrogen and normal pressure reaction atmosphere, and kept warm for 30-120 min; the nitrogen gas flow rate is 0.1-0.5 L / min; the heating rate is 5-10° C. / min;
[0010] Furthermore, the product after the reaction is washed, filtered and dried to obtain hexagonal boron nitride nanosheets h-BNNS;
[0011] Further, the product after the reaction is mixed with deionized water, heated to 60-90° C., stirred until the molten salt is completely dissolved, and then filtered, and the solid obtained by filtration is dried at a temperature of 80-120° C. for 2-4 hours to obtain hexagonal boron nitride nanosheets h-BNNS;
[0012] Further, the solution obtained by suction filtration is heated and evaporated to obtain a recyclable molten salt;
[0013] Furthermore, the heating temperature is 100°C-120°C.
[0014] The beneficial effects of the present invention are as follows: the preparation method of the hexagonal boron nitride nanosheets of the present invention uses boron as a raw material, which is safer and non-toxic, environmentally friendly, and has low raw material prices compared to other bottom-up preparation methods using boron sources such as melamine, ammonia borane, and borazane. The preparation method of the present invention is simple to operate and does not require large-scale equipment. It can not only prepare high-purity h-BNNS, but also recycle molten salt, thereby achieving the purpose of saving economic costs and reducing emissions, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0016] Figure 1 Flow chart for preparation
[0017] Figure 2 This is the X-ray diffraction pattern of h-BNNS prepared in Example 1.
[0018] Figure 3 This is a scanning electron microscope photograph of the h-BNNS prepared in Example 1.
[0019] Figure 4 This is a low-magnification transmission electron microscopy photograph of the h-BNNS prepared in Example 1.
[0020] Figure 5 This is a high-resolution transmission electron microscopy photograph of the h-BNNS prepared in Example 1. DETAILED DESCRIPTION
[0021] Embodiment 1
[0022] The method for preparing the hexagonal boron nitride nanosheets of this embodiment comprises the following steps:
[0023] Weigh 0.5g amorphous B powder, 2.5g NaCl and 2.5g KCl into an agate grinding mortar and grind for 30min until mixed evenly. Put the mixture of B powder and NaCl / KCl mixed salt into an alumina crucible, then place the crucible in a high-temperature furnace, evacuate to about -0.005MPa, and then introduce N2 to wash away the air in the furnace chamber (repeat the washing process twice). 0.5L / minN2 is introduced as a nitrogen source to make the furnace chamber at normal pressure, and the temperature is raised to 1400℃ at a heating rate of 10℃ / min. After keeping warm for 120min, it is cooled to room temperature with the furnace. Take out the product and transfer it to a beaker and add deionized water. Then place the beaker in a 90℃ water bath and use a magnetic stirrer for mechanical stirring for 10min to dissolve the molten salt in the product. Then, use a sand core filter to filter the stirred product to separate the salt solution and h-BNNS. The entire washing and filtration process is repeated 3 times. Finally, the filtered sample was placed in an oven and dried at 120°C for 2h to obtain dry h-BNNS. The filtered solution was transferred to a beaker, which was then placed on an electric furnace lined with asbestos mesh and heated to 100°C until the deionized water was completely evaporated to obtain recyclable molten salt.
[0024] Embodiment 2
[0025] The method for preparing the hexagonal boron nitride nanosheets of this embodiment comprises the following steps:
[0026] Weigh 0.5g amorphous B powder and 2.5g NaCl into an agate grinding mortar and grind for 15min until mixed evenly. Put the uniform mixture of B powder and NaCl into an alumina crucible, then place the crucible in a high-temperature furnace, evacuate to about -0.005MPa, and then introduce N2 to wash away the air in the furnace chamber (repeat the washing process 3 times). 0.3L / min N2 is introduced as a nitrogen source to make the furnace chamber at normal pressure, and the temperature is raised to 1200℃ at a heating rate of 8℃ / min. After keeping warm for 60min, it is cooled to room temperature with the furnace. Take out the product and transfer it to a beaker and add deionized water. Then place the beaker in a water bath at 80℃ and use a magnetic stirrer for mechanical stirring for 20min to dissolve the molten salt in the product. Then, use a sand core filter to filter the stirred product to separate the salt solution and h-BNNS. The entire washing and filtration process is repeated twice. Finally, the filtered sample was placed in an oven and dried at 100°C for 3 h to obtain dry h-BNNS. The filtered solution was transferred to a beaker, which was then placed on an electric furnace lined with asbestos mesh and heated to 110°C for insulation until the deionized water was completely evaporated to obtain recyclable molten salt.
[0027] Embodiment 3
[0028] The method for preparing the hexagonal boron nitride nanosheets of this embodiment comprises the following steps:
[0029] Weigh 0.5g amorphous B powder and 0.5g KCl into a ball mill and grind for 10min until mixed evenly. Put the uniform mixture of B powder and KCl into an alumina crucible, then place the crucible in a high-temperature furnace, evacuate to about -0.005MPa, and then introduce N2 to wash away the air in the furnace chamber (repeat the washing process 3 times). 0.1L / min N2 is introduced as a nitrogen source to make the furnace chamber at normal pressure, and the temperature is raised to 1000℃ at a heating rate of 5℃ / min. After keeping warm for 30min, it is cooled to room temperature with the furnace. Take out the product and transfer it to a beaker and add deionized water. Then place the beaker in a 60℃ water bath and use a magnetic stirrer for mechanical stirring for 10min to dissolve the molten salt in the product. Then, use a sand core filter to filter the stirred product to separate the salt solution and h-BNNS. The entire washing and filtration process is repeated 4 times. Finally, the filtered sample was placed in an oven and dried at 80°C for 4 hours to obtain dry h-BNNS. The filtered solution was transferred to a beaker, which was then placed on an electric furnace lined with asbestos mesh and heated to 120°C for insulation until the deionized water was completely evaporated to obtain recyclable molten salt.
[0030] Embodiment 4
[0031] The method for preparing the hexagonal boron nitride nanosheets of this embodiment comprises the following steps:
[0032] Weigh 0.5g amorphous B powder, 0.75g NaCl and 0.25g KCl into an agate grinding mortar and grind for 30min until mixed evenly. Put the mixture of B powder and NaCl / KCl mixed salt into an alumina crucible, then transfer the crucible into a high-temperature furnace, evacuate to about -0.005MPa, and then introduce N2 to wash away the oxygen in the furnace chamber (repeat the washing process 3 times). 0.5L / min N2 is introduced as a nitrogen source to make the furnace chamber at normal pressure, and the temperature is raised to 1400℃ at a heating rate of 10℃ / min. After keeping warm for 120min, it is cooled to room temperature with the furnace. Take out the product and transfer it to a beaker and add deionized water. Then place the beaker in a 90℃ water bath and use a magnetic stirrer for mechanical stirring for 10min to dissolve the molten salt in the product. Then, use a sand core filter to filter the stirred product to separate the molten salt solution and h-BNNS. The entire washing and filtration process is repeated 3 times. Finally, the filtered sample was placed in an oven and dried at 120°C for 2 h to obtain dry h-BNNS. The filtered solution was transferred to a beaker, and the beaker was placed on an electric furnace with an asbestos mesh and heated to 120°C for insulation until the deionized water was completely evaporated to obtain a recyclable molten salt.
[0033] In the above embodiments, the effects of embodiments 2-4 are better than those of embodiment 1.
[0034] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing hexagonal boron nitride nanosheets, characterized in that: The following steps are involved: Boron powder and molten salt are mixed and synthesized at high temperature under nitrogen conditions, and the synthesized product is separated to obtain hexagonal boron nitride nanosheets h-BNNS and recyclable molten salt.
2. The method for preparing hexagonal boron nitride nanosheets according to claim 1, characterized in that: The ratio of the molten salt to the boron powder is 1:1-10:
1.
3. The method for preparing hexagonal boron nitride nanosheets according to claim 2, characterized in that: The molten salt is pure sodium chloride, pure potassium chloride or a mixture of the two.
4. The method for preparing hexagonal boron nitride nanosheets according to claim 1, characterized in that: Boron powder and molten salt are mixed by mechanical grinding to obtain mixed powder, and the grinding time is 10-30 minutes.
5. The method for preparing hexagonal boron nitride nanosheets according to claim 1, characterized in that: The mixed powder is heated to 1000-1400° C. in a nitrogen and normal pressure reaction atmosphere, and kept warm for 30-120 minutes; the nitrogen gas flow rate is 0.1-0.5 L / min; and the heating rate is 5-10° C. / min.
6. The method for preparing hexagonal boron nitride nanosheets according to claim 1, characterized in that: The product after the reaction is washed, filtered and dried to obtain hexagonal boron nitride nanosheets h-BNNS.
7. The preparation method of hexagonal boron nitride nanosheets according to claim 6, characterized in that: The product after the reaction is mixed with deionized water, heated to 60-90° C., stirred until the molten salt is completely dissolved, and then filtered. The solid obtained by filtration is dried at a temperature of 80-120° C. for 2-4 hours to obtain hexagonal boron nitride nanosheets h-BNNS.
8. The method for preparing hexagonal boron nitride nanosheets according to claim 7, characterized in that: The filtered solution is heated and evaporated to obtain recyclable molten salt.
9. The method for preparing hexagonal boron nitride nanosheets according to claim 8, characterized in that: The heating temperature is 100℃-120℃.
Citation Information
Patent Citations
Boron nitride nanosheet powder, green macroscopic preparation method and application thereof
CN107585749A
Boron nitride nanosheet powder and low-cost batch preparation method thereof
CN107640750A
Low-temperature synthesis rhombic boron nitride powder based on fused salt method and preparation method thereof
CN108483414A
High-purity boron nitride nanotube and preparation method thereof
CN113336202A
Rare earth element doped WS2 nanosheet as well as preparation method and application thereof