Clustered ZSM-4 molecular sieve as well as preparation method and application thereof

By adding cationic solution in the synthesis of ZSM-4 molecular sieve to control crystal nucleation and growth to form a cluster structure, it solves the problems of traditional ZSM-4 molecular sieve catalyst deactivation and crystal size less than 100nm, and achieves higher catalytic performance and reaction efficiency. .

CN118791012APending Publication Date: 2024-10-18CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310403912.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The microporous channel structure of the existing ZSM-4 molecular sieve causes rapid deactivation of the catalyst, and there are few synthesis documents with crystal sizes less than 100 nm, making it difficult to overcome the diffusion limitations of traditional zeolite molecular sieves.

Method used

By adding cationic solution to control the crystal nucleation growth time and the size of individual crystals, hydrothermal crystallization and roasting are used to synthesize clustered ZSM-4 molecular sieves, and multiple nanoneedle-shaped single crystals are ordered and superimposed to form clusters, which can be expanded pore size and improved catalytic performance.

Benefits of technology

It achieves rapid nucleation and crystallization, extends the catalyst life, improves the external specific surface area and catalytic ability of the molecular sieve, and is suitable for the lightening reaction of m-trimethylbenzene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791012A_ABST
    Figure CN118791012A_ABST
Patent Text Reader

Abstract

The invention relates to a clustered ZSM-4 molecular sieve as well as a preparation method and application thereof. Comprising the following steps: S1, mixing an aluminum source, a buffer agent, an alkali source, water and a first metal cation compound to obtain a first mixture; s2, mixing the first mixture, a silicon source and a template agent to obtain a second mixture; s3, performing hydrothermal crystallization treatment and first roasting treatment on the second mixture to obtain an intermediate product; and S4, mixing the intermediate product with a second metal cation compound, and carrying out second roasting treatment. The nucleation growth of the crystals can be controlled and the morphology and size of a single crystal can be regulated and controlled by adding a compound containing metal cations as a growth promoting agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of molecular sieves, and in particular, to a clustered ZSM-4 molecular sieve and a preparation method and application thereof. Background Art

[0002] Zeolite molecular sieves are widely used in oil refining and petrochemical processes (such as catalytic cracking, hydrocracking, isomerization, etc.) to produce high-value final chemical products due to their unique pore structure, acidity and stability under harsh processing conditions. Although the traditional oil refining and petrochemical industries are currently committed to the transformation from mainly producing transportation fuels to producing value-added chemicals, due to the diversity and adjustable properties of zeolite molecular sieve structures, molecular sieve materials will still have an important impact in this field.

[0003] ZSM-4 molecular sieve has a MAZ topological structure and is a hexagonal crystal system with unit cell parameters. It has a one-dimensional 12-membered ring straight-through channel system with a crystallographic free diameter of Not connected to other pore systems; two-dimensional 8-membered ring pore system (crystallographic free diameter is ) and a one-dimensional 8-membered ring channel system (crystallographic free diameter is ) are interconnected, but their diameter is too small, which basically limits the molecular diffusion behavior.

[0004] The closed channels and cage-like structures of microporous zeolite molecular sieves always bring about mass transfer limitations in catalytic or separation applications. Their narrow pore size and long diffusion path will lead to rapid catalyst deactivation due to carbon deposition, which is more obvious in zeolite molecular sieves with low-dimensional pores. Therefore, overcoming the inherent transport limitations of microporous channels is an important goal in the field of zeolite molecular sieve design and synthesis. Although there are many literatures showing that the preparation of nanocrystals can improve the life of zeolite molecular sieve catalysts and / or change the selectivity of products by reducing internal diffusion limitations, there are still few reports on the synthesis of zeolite molecular sieves with crystal sizes less than 100nm.

[0005] Agglomerated, self-assembled or ordered nano-zeolite molecular sieves can form a rich intercrystalline pore system through spatial stacking. The free diameter of these intercrystalline pores is usually between 2 and 100 nm, which is between the mesopore and macropore size range. These intercrystalline pores and the micropores inherent in the molecular sieve zeolite matrix have different scale characteristics and different and complementary functions. The micropores below 1 nm are shape-selective for guest molecules with larger dynamic sizes, while the mesopores and macropores between crystals can improve the diffusion performance of guest molecules.

[0006] US3642434 first disclosed a method for synthesizing ZSM-4 molecular sieves, using tetramethylammonium chloride as a template agent, and the target product can be prepared within 7 to 15 days; JP2012161786 discloses a method for preparing seeds first by tetramethylammonium hydroxide within 10 days, and then secondary synthesis of MAZ type molecular sieves. None of the above patents involve cluster nanoparticles and pore structures with different scale characteristics, and the synthesis time is too long. CN112047357A reports a method for preparing Omega molecular sieves by choline, but the molecular sieve obtained has a large single crystal form and disordered clusters. Summary of the invention

[0007] The purpose of the present disclosure is to provide a clustered ZSM-4 molecular sieve and a preparation method and application thereof, which can control the crystal nucleation growth time and regulate the morphology and size of a single crystal by adding a cationic solution.

[0008] In order to achieve the above object, the present disclosure provides a method for preparing a clustered ZSM-4 molecular sieve in a first aspect, comprising the following steps:

[0009] S1, mixing an aluminum source, a buffer, an alkali source, water and a first metal cation compound to obtain a first mixture;

[0010] S2, mixing the first mixture, a silicon source and a template to obtain a second mixture;

[0011] S3, subjecting the second mixture to a hydrothermal crystallization treatment and a first calcination treatment to obtain an intermediate product;

[0012] S4, mixing the intermediate product with a second metal cation compound and performing a second calcination treatment. Optionally, the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water is (0.001-1):1:(0.02-1):(0.02-1):(0.01-1):(0.005-0.8):(10-200);

[0013] Preferably, the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water is (0.05-0.8):1:(0.05-0.5):(0.04-0.6):(0.05-0.5):(0.02-0.5):(10-60).

[0014] Optionally, the aluminum source is selected from one or more of aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol, preferably aluminum isopropoxide;

[0015] The buffer is selected from one or more of ammonium chloride, ammonium nitrate, ammonium bromide, ammonium fluoride and ammonium sulfate, preferably ammonium chloride;

[0016] The alkaline source is selected from one or more of sodium hydroxide, barium hydroxide, potassium hydroxide, ammonia water, sodium bicarbonate, sodium carbonate and potassium carbonate, preferably one or more of potassium hydroxide and ammonia water;

[0017] The silicon source is selected from one or more of silica sol, silica gel powder, white carbon black, water glass, methyl orthosilicate and ethyl orthosilicate, preferably one or more of silica sol, silica gel powder and water glass, and more preferably silica sol;

[0018] The template is selected from one or more quaternary ammonium base templates; preferably one or more selected from tetramethylammonium hydroxide, tetramethylammonium bromide, tetramethylammonium chloride, tetraethylammonium hydroxide, tetraethylammonium bromide and tetraethylammonium chloride.

[0019] Optionally, the first metal cation compound and the second metal cation compound are each independently selected from one or more of the hydroxides, nitrates, sulfates and chlorides of monovalent metals and divalent metals, preferably each independently selected from one or more of the nitrates, sulfates and chlorides of monovalent metals and divalent metals; further preferably, the first metal cation compound and the second metal cation compound are each independently selected from one or more of magnesium nitrate, magnesium chloride, magnesium sulfate, magnesium nitrate, calcium chloride, calcium sulfate, potassium nitrate, potassium chloride and potassium sulfate; further preferably, the first metal cation compound and the second metal cation compound are each independently selected from one or more of magnesium nitrate and calcium nitrate; optionally, the first metal cation compound and the second metal cation compound are the same or different, preferably the same;

[0020] Optionally, the first metal cation compound and the second metal cation compound are used in the form of a salt solution, and the concentration used is preferably 0.01 mol / L to 0.7 mol / L.

[0021] Optionally, in step S3, the conditions of the hydrothermal crystallization treatment include: a hydrothermal crystallization temperature of 80°C to 200°C, preferably 120°C to 200°C, and more preferably 130°C to 140°C; a hydrothermal crystallization time of 4h to 96h, preferably 10h to 48h, and more preferably 24h to 36h, and a pressure of autogenous pressure;

[0022] The conditions of the first calcination treatment include: a calcination temperature of 400°C to 650°C, preferably 500°C to 620°C, and more preferably 550°C to 600°C; and a calcination time of 3h to 12h, preferably 4h to 8h.

[0023] Optionally, in step S4, the solid-liquid mass volume ratio of the intermediate product to the second metal cation compound used in the form of a solution is 1:(1-200), preferably 1:(5-80);

[0024] Preferably, the conditions of the second calcination treatment include: a calcination temperature of 400°C to 650°C, preferably 500°C to 620°C, and more preferably 550°C to 600°C; and a calcination time of 3h to 12h, preferably 4h to 8h.

[0025] Optionally, the mixing of the intermediate product with the second metal cation compound in step S4 comprises:

[0026] The intermediate product is dispersed in deionized water, and after heating to 50° C. to 115° C., the second metal cation compound is added, and the pH of the slurry is controlled to be maintained in the range of 7 to 8 using a pH balancing agent, and then the water is removed;

[0027] Preferably, the pH balancing agent is selected from one or more of ammonia water, n-butylamine, citric acid, lactic acid, ethylenediaminetetraacetic acid and diethyltriaminepentaacetic acid.

[0028] The second aspect of the present disclosure provides a clustered ZSM-4 molecular sieve prepared according to the method described in the first aspect.

[0029] A third aspect of the present disclosure provides a clustered ZSM-4 molecular sieve, which includes a cluster body, and the cluster body includes a plurality of nano-needle-shaped single crystals.

[0030] Optionally, in the cluster, a plurality of nano needle-shaped single crystals are arranged in parallel;

[0031] Optionally, the average diameter of the nano needle-shaped single crystals is 50 nm to 80 nm.

[0032] Optionally, the total pore volume of the clustered ZSM-4 molecular sieve is 0.001 cm 3 / g~0.7cm 3 / g, preferably 0.01cm 3 / g~0.4cm 3 / g; micropore volume is 0.0005cm 3 / g~0.5cm 3 / g, preferably 0.001cm 3 / g~0.1cm 3 / g; mesopore volume is 0.0005cm 3 / g~0.6cm 3 / g, preferably 0.01cm 3 / g~0.3cm 3 / g; BET specific surface area is 10m 2 / g~400m 2 / g, preferably 60m 2 / g~270m 2 / g; the average pore diameter is 0.56nm to 50nm, preferably 2nm to 20nm.

[0033] The fourth aspect of the present disclosure provides the use of the clustered ZSM-4 molecular sieve described in the second and third aspects in the lightening reaction of meta-trimethylbenzene.

[0034] Optionally, the reaction conditions of the m-trimethylbenzene lightening reaction include: a temperature of 300°C to 600°C, preferably a temperature of 400°C to 550°C; a pressure of 0.001MPa to 2MPa, preferably a pressure of 0.005MPa to 1MPa, and more preferably a pressure of 0.01MPa to 0.5MPa; a mass space velocity of m-trimethylbenzene of 0.01h -1 ~10h -1 The preferred mass space velocity is 0.05h -1 ~5h -1 , more preferably the mass space velocity is 0.1h -1 ~2h -1 ;

[0035] Optionally, the meta-trimethylbenzene lightening reaction is carried out under carrier gas conditions, the carrier gas is selected from one or more of the inert gases, the volume flow rate of the carrier gas is 5mL / min to 100mL / min, preferably 10mL / min to 50mL / min, more preferably 10mL / min to 30mL / min; preferably, the inert gas includes N2.

[0036] Through the above technical solution, the present disclosure provides a clustered ZSM-4 molecular sieve and a preparation method and application thereof, which have at least the following beneficial effects:

[0037] (1) The present invention uses a compound containing a metal cation as a growth promoter, which is beneficial to the rapid nucleation of crystals, thereby increasing the crystallization rate and shortening the crystallization time;

[0038] (2) In the cationic promoter proposed in the present disclosure, divalent and higher cations can form charge balance with more framework atoms in the molecular sieve zeolite framework, thereby expanding the effective size of a single cage and making it easier for guest molecules to enter the pores and channels of the resulting molecular sieve;

[0039] (3) The pH balancing reagents used in the present disclosure do not contain inorganic metal ions, which can effectively avoid their interference with the growth promoter; at the same time, the pH balancing reagent can be removed in the subsequent roasting process without affecting the morphology, structure and function of the target product ZSM-4 molecular sieve;

[0040] (4) The preparation method provided by the present invention can synthesize a single nanorod-shaped single crystal with a diameter less than 100 nm. Multiple nanoneedle-shaped crystals are stacked into clusters through orderly stacking (arranged in an orderly manner approximately in parallel). The stacking gap of the nanoneedles is 2 to 5 nm, which belongs to the mesoporous range. The morphology of the ZSM-4 zeolite molecular sieve is improved, and it has a higher external specific surface area and good adsorption and catalytic capabilities.

[0041] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0043] Figure 1 This is the SEM image of the product obtained in Comparative Example 1;

[0044] Figure 2 This is the SEM image of the molecular sieve obtained in Example 1;

[0045] Figure 3 This is the SEM image of the molecular sieve obtained in Example 2;

[0046] Figure 4 This is a SEM image of the molecular sieve obtained in Example 3;

[0047] Figure 5 This is a SEM image of the molecular sieve obtained in Example 4;

[0048] Figure 6 This is a SEM image of the molecular sieve obtained in Example 5;

[0049] Figure 7 This is the SEM image of the molecular sieve obtained in Example 6;

[0050] Figure 8a This is the SEM image of the molecular sieve obtained in Example 7;

[0051] Figure 8b This is the SEM image of the molecular sieve obtained in Example 7;

[0052] Fig. 9 The nitrogen adsorption and desorption curves of the molecular sieves obtained in Comparative Example 1 and Examples 4 to 7 are shown;

[0053] Fig.10 This is the XRD pattern of the molecular sieve obtained in Example 7. DETAILED DESCRIPTION

[0054] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.

[0055] The inventors of the present disclosure have discovered through a large number of experimental studies that cations with larger diameters cannot enter the small-size pore structure of the molecular sieve to balance the negative charge caused by the four skeleton aluminum atoms because their size is larger than the inherent 8-membered ring crystallographic free diameter. This can cause aluminum to be preferentially enriched in the 12-membered ring pores, so that the 12-membered ring pores of the molecular sieve not only have abundant catalytic reaction active sites, but also have a larger crystallographic free diameter, which is convenient for most guest molecules present in the catalytic process of oil refining and petrochemicals to react and diffuse.

[0056] The first aspect of the present disclosure provides a method for preparing a clustered ZSM-4 molecular sieve, comprising the following steps:

[0057] S1, mixing an aluminum source, a buffer, an alkali source, water and a first metal cation compound to obtain a first mixture;

[0058] S2, mixing the first mixture, a silicon source and a template to obtain a second mixture;

[0059] S3, subjecting the second mixture to a hydrothermal crystallization treatment and a first calcination treatment to obtain an intermediate product;

[0060] S4, mixing the intermediate product with a second metal cation compound and performing a second calcination treatment.

[0061] The present disclosure provides a method for preparing a clustered ZSM-4 molecular sieve, using a compound containing a metal cation as a growth promoter, which is conducive to the rapid nucleation of crystals, thereby increasing the crystallization rate and shortening the crystallization time. The preparation method provided by the present disclosure can synthesize a single nanorod-shaped single crystal with a diameter less than 100nm, and a plurality of nanoneedle-shaped single crystals are stacked into clusters by orderly superposition (arranged in an orderly manner approximately in parallel), and the nanoneedle stacking gap is 2 to 5nm, which belongs to the mesoporous range, improves the morphology of the ZSM-4 zeolite molecular sieve, has a higher external specific surface area, and has good adsorption and catalytic capabilities.

[0062] In one embodiment, the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water is (0.001-1): 1: (0.02-1): (0.02-1): (0.01-1): (0.005-0.8): (10-200). In the present disclosure, the silicon source is calculated as SiO2, and the aluminum source is calculated as Al2O3.

[0063] In a preferred embodiment, the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water is (0.05-0.8): 1: (0.05-0.5): (0.04-0.6): (0.05-0.5): (0.02-0.5): (10-60). The molecular sieve is prepared according to the material molar ratio optimized in this embodiment, and a ZSM-4 cluster molecular sieve with better performance can be obtained.

[0064] In a specific embodiment, in step S2, a mixed alkali source may be added, and the types of alkali sources in steps S2 and S1 may be the same or different; the alkali source in the molar ratio when the raw materials are mixed is calculated according to the amount of all alkali sources added.

[0065] In a specific embodiment, the aluminum source is selected from one or more of aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol, preferably aluminum isopropoxide;

[0066] The buffer is selected from one or more of ammonium chloride, ammonium nitrate, ammonium bromide, ammonium fluoride and ammonium sulfate, preferably ammonium chloride;

[0067] The alkali source is selected from one or more of sodium hydroxide, barium hydroxide, potassium hydroxide, ammonia water, sodium bicarbonate, sodium carbonate and potassium carbonate, preferably one or more of potassium hydroxide and ammonia water;

[0068] The silicon source is selected from one or more of silica sol, silica gel powder, white carbon black, water glass, methyl orthosilicate and ethyl orthosilicate, preferably one or more of silica sol, silica gel powder and water glass, and more preferably silica sol;

[0069] The template is selected from one or more quaternary ammonium base templates; preferably one or more selected from tetramethylammonium hydroxide, tetramethylammonium bromide, tetramethylammonium chloride, tetraethylammonium hydroxide, tetraethylammonium bromide and tetraethylammonium chloride.

[0070] Various reagents used in the present disclosure can be purchased through conventional channels or prepared by known methods.

[0071] In one embodiment, the first metal cation compound and the second metal cation compound are each independently selected from one or more of the hydroxides, nitrates, sulfates and chlorides of monovalent metals and divalent metals, preferably each independently selected from one or more of the nitrates, sulfates and chlorides of monovalent metals and divalent metals; further preferably, the first metal cation compound and the second metal cation compound are each independently selected from one or more of magnesium nitrate, magnesium chloride, magnesium sulfate, magnesium nitrate, calcium chloride, calcium sulfate, potassium nitrate, potassium chloride and potassium sulfate; further preferably, the first metal cation compound and the second metal cation compound are each independently selected from one or more of magnesium nitrate and calcium nitrate; optionally, the first metal cation compound and the second metal cation compound are the same or different, preferably the same. In the cationic growth promoter provided in this embodiment, the preferred divalent and higher cation salts can form a charge balance with more framework atoms in the molecular sieve zeolite framework, thereby expanding the effective size of a single cage and making it easier for guest molecules to enter the pores and channels.

[0072] In a preferred embodiment, the cation diameters of the first metal cation compound and the second metal cation compound are the following.

[0073] In a specific embodiment, the first metal cation compound and the second metal cation compound are used in the form of a salt solution, and the concentration used is preferably 0.01 mol / L to 0.7 mol / L.

[0074] In one embodiment, in step S3, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization temperature is 80°C to 200°C, preferably 120°C to 200°C, and more preferably 130°C to 140°C; the hydrothermal crystallization time is 4h to 96h, preferably 10h to 48h, and more preferably 24h to 36h, and the pressure is autogenous pressure;

[0075] The conditions of the first calcination treatment include: a calcination temperature of 400°C to 650°C, preferably 500°C to 620°C, and more preferably 550°C to 600°C; a calcination time of 3h to 12h, preferably 4h to 8h. According to the optimized crystallization treatment conditions and calcination treatment conditions in this embodiment, it is beneficial to improve the structural performance of the molecular sieve.

[0076] In the present disclosure, the hydrothermal crystallization treatment and the calcination treatment are both carried out in conventional devices in the art.

[0077] In one embodiment, in step S4, the solid-liquid mass volume ratio of the intermediate product to the second metal cation compound solution is 1:(1-200), preferably 1:(5-80).

[0078] In one embodiment, in step S4, the conditions of the second calcination treatment include: a calcination temperature of 400°C to 650°C, preferably 500°C to 620°C, and more preferably 550°C to 600°C; and a calcination time of 3h to 12h, preferably 4h to 8h.

[0079] In a specific embodiment, the mixing of the intermediate product with the second metal cation compound in step S4 comprises:

[0080] The intermediate product is dispersed in deionized water, heated to 50°C to 115°C, the second metal cation compound is added, a pH balance reagent is used to control the pH of the slurry to be maintained in the range of 7 to 8, and then the water is removed. Specifically, the method of removing water may include: continuously rotating in a rotary evaporator until evaporated to dryness.

[0081] In one embodiment, the pH balancing agent is selected from one or more of ammonia water, n-butylamine, citric acid, lactic acid, ethylenediaminetetraacetic acid and diethyltriaminepentaacetic acid. The solution balancing agents used in the present disclosure do not contain inorganic metal ions, which can effectively avoid their interference with the growth promoter. At the same time, the balancing agent can be removed in the subsequent roasting process without affecting the morphology, structure and function of the target product ZSM-4 molecular sieve.

[0082] The second aspect of the present disclosure provides a clustered ZSM-4 molecular sieve prepared according to the method described in the first aspect.

[0083] A third aspect of the present disclosure provides a clustered ZSM-4 molecular sieve, which includes a cluster body, and the cluster body includes a plurality of nano-needle-shaped single crystals.

[0084] In the present disclosure, clusters are obtained by arranging a plurality of nano-needle-shaped single crystals in an orderly manner in roughly parallel manner; and through a scanning electron microscope, it can be seen that the molecular sieve sample can include a plurality of clusters in different directions, and through ultrasonic vibration and other means, the clusters in different directions can be arranged in roughly the same direction.

[0085] In the present disclosure, in the cluster, the stacking gap between two adjacent nano needle-shaped single crystals is 2nm to 5nm. The stacking gap between two adjacent nano needle-shaped single crystals in the present disclosure is measured by a scanning electron microscope method.

[0086] In one embodiment, the average diameter of the nano needle-shaped single crystals is 50 nm to 80 nm.

[0087] In one specific embodiment, the total pore volume of the clustered ZSM-4 molecular sieve is 0.001 cm 3 / g~0.7cm 3 / g, preferably 0.01cm 3 / g~0.4cm 3 / g; micropore volume is 0.0005cm 3 / g~0.5cm 3 / g, preferably 0.001cm 3 / g~0.1cm 3 / g; mesopore volume is 0.0005cm 3 / g~0.6cm 3 / g, preferably 0.01cm 3 / g~0.3cm 3 / g; BET specific surface area is 10m 2 / g~400m 2 / g, preferably 60m 2 / g~270m 2 / g; the average pore diameter is 0.56nm to 50nm, preferably 2nm to 20nm.

[0088] The fourth aspect of the present disclosure provides the use of the clustered ZSM-4 molecular sieve described in the second or third aspect of the present disclosure in the lightening reaction of meta-trimethylbenzene.

[0089] In a specific embodiment, the reaction conditions of the meta-trimethylbenzene lightening reaction include: a temperature of 300°C to 600°C, preferably a temperature of 400°C to 550°C; a pressure of 0.001MPa to 2MPa, preferably a pressure of 0.005MPa to 1MPa, and more preferably a pressure of 0.01MPa to 0.5MPa; a mass space velocity of meta-trimethylbenzene of 0.01h -1 ~10h -1 The preferred mass space velocity is 0.05h -1 ~5h -1 , more preferably the mass space velocity is 0.1h -1 ~2h -1 ;

[0090] Optionally, the meta-trimethylbenzene lightening reaction is carried out under carrier gas conditions, the carrier gas is selected from one or more of the inert gases, the volume flow rate of the carrier gas is 5mL / min to 100mL / min, preferably 10mL / min to 50mL / min, more preferably 10mL / min to 30mL / min; preferably, the inert gas includes N2.

[0091] The present disclosure is further described in detail by way of examples. The raw materials used in the examples can all be obtained through commercial sources.

[0092] In the following embodiments, when calculating the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: water, the amount of water is based on the total amount of water added when the raw materials are mixed (before crystallization treatment) (including deionized water added together with the aluminum source and deionized water added subsequently).

[0093] In the following examples, the first metal cation compound and the second metal cation compound are the same type of cation compounds.

[0094] Example 1

[0095] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.16:1:0.11:0.081:0.07:0.11:13.5, the aluminum sol (calculated as Al2O3) was dissolved in 30g of deionized water and gradually heated to 55°C, and 1mol / L ammonium chloride solution and 0.009mol / L ammonia water were added. After the solution was mixed evenly, the magnesium hydroxide powder added was stirred for 30min. Turn off the heating and add the silica sol (calculated as SiO2) at one time. When a gel appears during the addition process, increase the stirring rate and add deionized water in time, and a total of 13.4g of deionized water is added. After it becomes emulsion-like, tetramethylammonium hydroxide is added dropwise and stirred continuously, and then transferred to a high-pressure hydrothermal reactor for crystallization at 120°C for 48h. After the crystallization is completed, the reactor is placed in a water tank for cooling. The cooled product is separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reaches neutral. The filter cake was dried at 120℃ for 12h, ground and crushed, and calcined at 590℃ for 5h to obtain molecular sieve powder (intermediate product). 0.5mol / L magnesium hydroxide suspension was added, and the molecular sieve mass: cationic suspension volume was 1:10. The two were evenly mixed, and 0.01mol / L citric acid was added dropwise to keep the pH of the molecular sieve suspension at about 8. The mixture was transferred to a rotary evaporator, heated to 75℃ and rotated continuously until evaporated. The evaporated powder was ground and calcined at 550℃ for 5h to obtain a molecular sieve product, which was recorded as C-1.

[0096] Example 2

[0097] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.35:1:0.11:0.30:0.15:0.36:68, aluminum sulfate was dissolved in 19g of deionized water and gradually heated to 55°C, 1mol / L ammonium chloride solution and 0.009mol / L ammonia water were added, and then stirring was continued and 0.5mol / L magnesium chloride solution was added. Turn off the heating, and after cooling to room temperature, water glass (based on SiO2) was slowly added. After rapid stirring to an emulsion, 10g of deionized water was added, and tetramethylammonium bromide was added dropwise. The mixed emulsion was transferred to a high-pressure hydrothermal reactor for crystallization at 140°C for 48h. After the crystallization was completed, the reactor was placed in a water tank for cooling. The cooled product was separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reached neutral. The filter cake was dried at 120℃ for 12h, ground and crushed, and calcined at 590℃ for 5h to obtain molecular sieve powder (intermediate product). According to the molecular sieve mass: 0.5mol / L cationic aqueous solution (magnesium chloride solution) volume of 1:10, the two were evenly mixed, and 0.1mol / L ammonia water was added dropwise to keep the pH of the molecular sieve suspension at about 8, and transferred to a rotary evaporator, heated to 75℃ and rotated continuously until evaporated. The evaporated powder was ground and calcined at 550℃ for 5h to obtain a molecular sieve product, recorded as C-2.

[0098] Example 3

[0099] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.18:1:0.06:0.13:0.11:0.23:10.45, aluminum nitrate and potassium hydroxide powder are first added to 20g of deionized water at 60°C and mixed evenly, and stirring is maintained. 1mol / L ammonium chloride solution and 0.009mol / L ammonia water and 0.5mol / L magnesium nitrate solution are added, wherein the molar ratio of potassium hydroxide powder to ammonia water is 0.30:1. After stirring for 30min, the heating is turned off, and silica sol (based on SiO2) is added dropwise and the stirring rate is increased. After adding 9g of deionized water, tetramethylammonium hydroxide is added, and the mixed emulsion is transferred to a high-pressure hydrothermal reactor for crystallization at 140°C for 24h. After the crystallization is completed, the reactor is placed in a water tank for cooling. The cooled product is separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reaches neutral. The filter cake was dried at 120℃ for 12h, ground and crushed, and calcined at 590℃ for 5h to obtain molecular sieve powder (intermediate product). According to the molecular sieve mass: 0.5mol / L cationic aqueous solution (magnesium nitrate solution) volume of 1:10, the two were evenly mixed, 0.1mol / L citric acid was added dropwise to keep the pH of the molecular sieve suspension at about 8, and transferred to a rotary evaporator, heated to 75℃ and rotated continuously until evaporated. The evaporated powder was ground and calcined at 550℃ for 5h to obtain a molecular sieve product, recorded as C-3.

[0100] Example 4

[0101] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.07:1:0.11:0.04:0.07:0.15:15, aluminum sol (calculated as Al2O3) and potassium hydroxide powder were dissolved in 12g of deionized water, stirred continuously and heated to 50°C. After mixing evenly, 1mol / L ammonium chloride solution, concentrated ammonia water and calcium hydroxide powder were added, wherein the molar ratio of potassium hydroxide powder to ammonia water was 0.30:1. After adding 20g of deionized water and stirring continuously for 30min, silica sol (calculated as SiO2) was added dropwise, and tetramethylammonium hydroxide was added. When a gel appeared during the mixing process, the stirring rate was increased in time. After adding 6.6g of deionized water, the mixed emulsion was transferred to a high-pressure hydrothermal reactor for crystallization at 140°C for 24h. After the crystallization was completed, the reactor was placed in a water tank for cooling. The cooled product was separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reached neutral. The filter cake was dried at 120°C for 12 hours, ground and crushed, and calcined at 590°C for 5 hours to obtain a molecular sieve powder (intermediate product). According to the molecular sieve mass: 0.5 mol / L cationic suspension (calcium hydroxide suspension) volume of 1:10, the two were evenly mixed, and 0.02 mol / L citric acid aqueous solution was added dropwise to keep the pH of the molecular sieve suspension at about 8, and transferred to a rotary evaporator, heated to 75°C and rotated continuously until evaporated to dryness. The evaporated powder was ground and calcined at 550°C for 5 hours to obtain a molecular sieve product, recorded as C-4.

[0102] Example 5

[0103] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.6:1:0.32:0.52:0.39:0.44:56, aluminum isopropoxide and potassium hydroxide powder are dissolved in 17.5g deionized water, heated to 65°C, 1mol / L ammonium chloride solution and potassium hydroxide are added (the molar ratio of potassium hydroxide before and after is 7:1), and 0.5mol / L calcium sulfate solution is added during continuous stirring. After stirring for 30min, the heating is stopped, and after cooling to room temperature, ethyl orthosilicate is added dropwise. When a gel appears during the addition process, the stirring rate is increased in time, 3g deionized water is added, and tetramethylammonium bromide is added dropwise. The mixed emulsion is transferred to a high-pressure hydrothermal reactor for crystallization at 140°C for 24h. After the crystallization is completed, the reactor is placed in a water tank for cooling. The cooled product is separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reaches neutral. The filter cake was dried at 120℃ for 12h, ground and crushed, and calcined at 590℃ for 5h to obtain molecular sieve powder (intermediate product). According to the molecular sieve mass: 0.5mol / L cationic aqueous solution (calcium sulfate solution) volume of 1:10, the two were evenly mixed, and 0.1mol / L ammonia water was added dropwise to keep the pH of the molecular sieve suspension at about 8, and transferred to a rotary evaporator, heated to 75℃ and rotated continuously until evaporated. The evaporated powder was ground and calcined at 550℃ for 5h to obtain a molecular sieve product, recorded as C-5.

[0104] Example 6

[0105] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.088:1:0.11:0.04:0.05:0.15:20, aluminum sol (calculated as Al2O3) and potassium hydroxide powder were dissolved in 27.5g deionized water, heated to 55°C, 1mol / L ammonium chloride solution and ammonia water were added, the molar ratio of potassium hydroxide powder to ammonia water was 0.20:1, stirring continuously, and 0.5mol / L calcium chloride solution was added. After stirring for 30min, heating was stopped, and after cooling to room temperature, silica sol (calculated as SiO2) was added dropwise. When a gel appeared during the addition process, the stirring rate was increased in time, and 4g deionized water and tetramethylammonium hydroxide were added. The mixed emulsion was transferred to a high-pressure hydrothermal reactor for crystallization at 140°C for 24h. After the crystallization was completed, the reactor was placed in a water tank for cooling. The cooled product was separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reached neutral. The filter cake was dried at 120°C for 12 hours, ground and crushed, and calcined at 590°C for 5 hours to obtain a molecular sieve powder (intermediate product). According to the molecular sieve mass: 0.5 mol / L cationic aqueous solution (calcium chloride solution) volume of 1:10, the two were evenly mixed, 0.1 mol / L ammonia water was added dropwise to keep the pH of the molecular sieve suspension at about 8, and transferred to a rotary evaporator, heated to 75°C and rotated continuously until evaporated. The evaporated powder was ground and calcined at 550°C for 5 hours to obtain a molecular sieve product, recorded as C-6.

[0106] Example 7

[0107] According to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.088:1:0.11:0.04:0.05:0.15:20, aluminum sol (calculated as Al2O3) and potassium hydroxide powder were dissolved in 27.5g deionized water, heated to 55°C, 1mol / L ammonium chloride solution and ammonia water (the molar ratio of potassium hydroxide powder to ammonia water is 0.20:1) were added, and stirring was continued, followed by adding 70mL of 0.5mol / L calcium nitrate solution. After stirring for 30min, heating was stopped, and after cooling to room temperature, silica sol (calculated as SiO2) was added dropwise. When a gel appeared during the addition process, the stirring rate was increased in time, 4g of deionized water was added, and tetramethylammonium hydroxide was added dropwise. The well-mixed emulsion was transferred to a high-pressure hydrothermal reactor for crystallization at 140°C for 24h. After the crystallization was completed, the reactor was placed in a water tank for cooling. The cooled product was separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reached neutral. The filter cake was dried at 120°C for 12 hours, ground and crushed, and calcined at 590°C for 5 hours to obtain a molecular sieve powder (intermediate product). According to the molecular sieve mass: 0.5 mol / L cationic aqueous solution (calcium nitrate solution) volume of 1:10, the two were evenly mixed, 0.1 mol / L ammonia water was added dropwise to keep the pH of the molecular sieve suspension at about 8, and transferred to a rotary evaporator, heated to 75°C and rotated continuously until evaporated to dryness. The evaporated powder was ground and calcined at 550°C for 5 hours to obtain a molecular sieve product, recorded as C-7.

[0108] Example 8

[0109] Referring to the preparation method in Example 7, the difference from Example 7 is that the preparation is carried out according to the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water of 0.02:1:0.8:1:0.01:0.85:100, the type of raw materials and preparation conditions are the same as in Example 7, and a molecular sieve product is obtained, which is recorded as C-8.

[0110] Example 9

[0111] Referring to the preparation method in Example 7, the difference from Example 7 is that:

[0112] The conditions of the hydrothermal crystallization treatment are as follows: the hydrothermal crystallization temperature is 100°C; the hydrothermal crystallization time is 4h;

[0113] The conditions of the first calcination treatment include: calcination temperature of 500°C; calcination time of 3h, and molecular sieve powder (intermediate product) is obtained. According to the molecular sieve mass: 0.5mol / L cationic aqueous solution volume of 1:150, the two are evenly mixed, 0.1mol / L ammonia water is added dropwise to keep the pH of the molecular sieve suspension at about 8, and then transferred to a rotary evaporator, heated to 75°C and continuously rotated until evaporated. The evaporated powder is ground and calcined at 500°C for 3h to obtain a molecular sieve product, recorded as C-9.

[0114] Comparative Example 1

[0115] Dissolve 0.95g of aluminum isopropoxide in 6.4g of deionized water and gradually heat it to 55°C. Add 3.4mL of 1mol / L ammonium chloride solution and 0.46g of ammonia water, stir for 30min until uniform and stop heating. Then continue stirring and slowly add 6g of silica gel powder drop by drop. Add deionized water in time during the gel formation process. The amount of deionized water added is 69g. Add 0.64g of tetramethylammonium bromide and heat the emulsion to 45°C. After stirring evenly, put it into a high-pressure hydrothermal reactor and crystallize it at 120°C for 48h. After crystallization, place the reactor in a sink to cool. The cooled product is separated by suction filtration and repeatedly washed with deionized water until the pH value of the filtrate reaches neutral. The filter cake is dried at 120°C for 12h, ground and crushed, and calcined at 590°C for 5h to obtain a molecular sieve powder. Prepare 0.5 mol / L magnesium hydroxide suspension, mix the two evenly according to the molecular sieve mass: cationic suspension volume of 1:10, add 0.01 mol / L citric acid dropwise to keep the pH of the molecular sieve suspension at about 8, transfer to a rotary evaporator, heat to 75°C and continue rotating until evaporated to dryness. The evaporated powder is ground and calcined at 550°C for 5h to obtain a molecular sieve product, recorded as D-1.

[0116] Comparative Example 2

[0117] This comparative example refers to the preparation method in Example 1, and the difference from Example 1 is that the intermediate product is not mixed with the second metal cation compound, the second calcination treatment step is not performed, and only the intermediate product obtained in Example 1 is used as a molecular sieve sample, recorded as D-2.

[0118] Test Example 1

[0119] This test example is used to perform SEM characterization, XRD characterization and nitrogen adsorption-desorption characterization on the products prepared in the above examples and comparisons.

[0120] The SEM test used a JSM-7500F scanning electron microscope produced by Japan JEOL Company, with an operating voltage of 10 kV, a working distance of 7 mm, and a resolution of 1 nm.

[0121] The instrument used for XRD characterization is a PANalytical Empyrean X-ray diffractometer; the test method includes: the scanning range is set to 5° to 70°, the step length is 0.02°, and the scanning rate is 8° / min.

[0122] The conditions for nitrogen adsorption and desorption characterization refer to Test Example 2.

[0123] The SEM characterization results of the molecular sieves C-1 to C-7 and D-1 obtained in Examples 1 to 7 and Comparative Example 1 are as follows: Figure 1-8b As shown; Comparative Example 1 and Examples 4 to 7 obtained nitrogen adsorption and desorption curves of molecular sieves are shown Fig. 9 shown.

[0124] Depend on Figure 1 and Fig. 9 It can be seen that no cationic solution was added during the preparation process of Comparative Example 1, and the molecular sieve D-1 obtained in Comparative Example 1 was granular, only an amorphous product was obtained, and no molecular sieve was synthesized.

[0125] Examples 1 to 3 all use a growth promoter with magnesium as a cation to synthesize ZSM-4 molecular sieve. Figures 2 to 4 It can be seen from the comparison that in Example 1 using magnesium hydroxide as a promoter, only a small amount of cubic small crystals are synthesized, and there is no obvious MAZ type molecular sieve structure feature; in Example 2 using magnesium chloride as a promoter, thin strip-shaped ZSM-4 molecular sieve crystal structure begins to appear, but there is still a large amount of amorphous material; the MAZ crystal structure is clearly displayed in the SEM image of Example 3 using magnesium nitrate as a promoter.

[0126] In the molecular sieve synthesis process of Examples 4 to 7, a calcium-containing cationic compound was used as a growth promoter. The SEM photos of the products Figures 5 to 7 and Figure 8a-8b Obvious rod-like cluster crystal structures can be seen, indicating that the use of calcium-containing cationic compounds as promoters is conducive to the growth of straight-through ZSM-4 molecular sieve crystals.

[0127] Further, it can be seen from the SEM photos that the diameter of the single rod-shaped ZSM-4 molecular sieve (nano needle-shaped single crystal) obtained in Examples 4 to 7 is about 80nm, which is much smaller than the 200nm reported in existing literature or patents. The average diameter of the single rod-shaped ZSM-4 molecular sieve crystal (nano needle-shaped single crystal) obtained in the preferred Example 7 is only about 50nm, and the clusters presented after the single crystals are aggregated are ellipsoidal spheres. The crystal structure is clear in the SEM electron microscope image, and the single rod-shaped MAZ type molecular sieve crystal (nano needle-shaped single crystal) is more slender, with an average diameter of only 50nm, which improves the morphology of the zeolite molecular sieve, maintains a defect-free unit cell, good crystallinity and purity.

[0128] The XRD pattern of the molecular sieve C-7 prepared in Example 7 is as follows Fig.10 As shown by Fig.10 It can be seen that the XRD pattern of the molecular sieve C-7 has peaks at 2θ positions of 8.1, 11.9, 15.1, 16.2, 25.6, 27.6, 30.3, 31.1, 32.0, and 32.8, indicating that the molecular sieve prepared by the method provided in the present application has a ZSM-4 structure.

[0129] Test Example 2

[0130] This test example is used to characterize the structural properties of the products prepared in the above examples and comparisons. The specific test conditions include:

[0131] The specific surface area parameters and mesopore volume parameters were measured using the ASTM D4365 method; the instrument used was Micromeritics' AsAp 2400 static nitrogen adsorption instrument; the test process was as follows: the catalyst sample was degassed at 300 °C for 4 h to a vacuum degree of 1.33 × 10 -2 Pa, and then nitrogen is contacted with the adsorbent to be tested at liquid nitrogen temperature (-196°C) to reach static adsorption equilibrium, and the amount of nitrogen adsorbed by the adsorbent is calculated from the difference between the nitrogen intake and the amount remaining in the gas phase after adsorption. Then, the two-parameter BET formula is used to calculate the specific surface area and pore volume, and the BJH formula is used to calculate the pore size distribution and the corresponding mesopore volume.

[0132] The structural parameters of the molecular sieve products prepared in some of the above examples and comparisons are listed in the following Table 1.

[0133] Table 1

[0134]

[0135]

[0136] In Table 1, “-” means that the test was performed but the data of this item was not obtained.

[0137] Test Example 3

[0138] This test example is used to test the catalytic performance of the products prepared in the above examples and comparative examples (application in the lightening reaction of meta-trimethylbenzene).

[0139] The reaction process includes: loading the molecular sieves prepared in the comparative example and the example into a small fixed bed reactor. The reaction conditions include: temperature of 550°C, pressure of 0.3 MPa, mass space velocity of m-trimethylbenzene of 0.5 h -1 The reaction time was 24 hours and the volume flow rate of nitrogen was 10 mL / min. The reaction results are listed in Table 2 below.

[0140] Wherein, 1,2,4-trimethylbenzene conversion rate (%) = (total mass of 1,2,4-trimethylbenzene input - mass of unreacted 1,2,4-trimethylbenzene) / total mass of 1,2,4-trimethylbenzene input × 100%;

[0141] Selectivity of light aromatics products (%) = total mass of benzene, toluene and xylene components in the product / total mass of the product × 100%;

[0142] Light aromatic product yield (%) = total mass of benzene, toluene and xylene components in the product / total mass of 1,2,4-trimethylolpropane input × 100%.

[0143] Table 2

[0144]

[0145]

[0146] According to the data in Table 2 above, it can be seen that compared with the products prepared in Comparative Examples 1 to 2, especially in Comparative Example 1 in which no first metal cation compound is added during the preparation process, the obtained product D-1 has no catalytic performance in the lightening reaction of meta-trimethylbenzene. The molecular sieve products C-1 to C-9 prepared by the method provided in the present application in Examples 1 to 8 have better catalytic performance in the lightening reaction of meta-trimethylbenzene, and the conversion rate of 1,2,4-trimethylbenzene, the selectivity of light aromatics products and the yield of light aromatics products are higher.

[0147] Comparing Example 7 with Example 8, it can be seen that in the molecular sieve preparation process of Example 7, the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water is (0.05-0.8):1:(0.05-0.5):(0.04-0.6):(0.05-0.5):(0.02-0.5):(10-60), and Example 8 is not within this optimized molar ratio range. The molecular sieve C-7 prepared in Example 7 has better catalytic performance than molecular sieve C-8 in the lightening reaction of meta-trimethylbenzene, and has higher 1,2,4-trimethylbenzene conversion rate, light aromatic product selectivity and light aromatic product yield.

[0148] By comparing Example 7 with Example 9, it can be seen that Example 7 adopts optimized preparation conditions in the molecular sieve preparation process, such as hydrothermal crystallization temperature and time, calcination temperature and time, etc. Compared with the molecular sieve C-9 obtained in Example 9, the molecular sieve C-7 prepared in Example 7 has better catalytic performance in the lightening reaction of meta-trimethylbenzene, and has higher 1,2,4-trimethylbenzene conversion rate, light aromatic product selectivity and light aromatic product yield.

[0149] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0150] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0151] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A method for preparing a clustered ZSM-4 molecular sieve, characterized in that: The following steps are involved: S1, mixing an aluminum source, a buffer, an alkali source, water and a first metal cation compound to obtain a first mixture; S2, mixing the first mixture, a silicon source and a template to obtain a second mixture; S3, subjecting the second mixture to a hydrothermal crystallization treatment and a first calcination treatment to obtain an intermediate product; S4, mixing the intermediate product with a second metal cation compound and performing a second calcination treatment.

2. The method according to claim 1, characterized in that The molar ratio of the first metal cation compound: silicon source: aluminum source: template agent: buffer agent: alkali source: water is (0.001-1):1:(0.02-1):(0.02-1):(0.01-1):(0.005-0.8):(10-200); Preferably, the molar ratio of the first metal cation compound: silicon source: aluminum source: template: buffer: alkali source: water is (0.05-0.8):1:(0.05-0.5):(0.04-0.6):(0.05-0.5):(0.02-0.5):(10-60).

3. The method according to claim 1, characterized in that The aluminum source is selected from one or more of aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol, preferably aluminum isopropoxide; The buffer is selected from one or more of ammonium chloride, ammonium nitrate, ammonium bromide, ammonium fluoride and ammonium sulfate, preferably ammonium chloride; The alkali source is selected from one or more of sodium hydroxide, barium hydroxide, potassium hydroxide, ammonia water, sodium bicarbonate, sodium carbonate and potassium carbonate, preferably one or more of potassium hydroxide and ammonia water; The silicon source is selected from one or more of silica sol, silica gel powder, white carbon black, water glass, methyl orthosilicate and ethyl orthosilicate, preferably one or more of silica sol, silica gel powder and water glass, and more preferably silica sol; The template is selected from one or more quaternary ammonium base templates; preferably one or more selected from tetramethylammonium hydroxide, tetramethylammonium bromide, tetramethylammonium chloride, tetraethylammonium hydroxide, tetraethylammonium bromide and tetraethylammonium chloride.

4. The method according to claim 1, characterized in that: The first metal cation compound and the second metal cation compound are each independently selected from one or more of the hydroxides, nitrates, sulfates and chlorides of monovalent metals and divalent metals, preferably each independently selected from one or more of the nitrates, sulfates and chlorides of monovalent metals and divalent metals; further preferably, the first metal cation compound and the second metal cation compound are each independently selected from one or more of magnesium nitrate, magnesium chloride, magnesium sulfate, magnesium nitrate, calcium chloride, calcium sulfate, potassium nitrate, potassium chloride and potassium sulfate; further preferably, the first metal cation compound and the second metal cation compound are each independently selected from one or more of magnesium nitrate and calcium nitrate; optionally, the first metal cation compound and the second metal cation compound are the same or different, preferably the same; Optionally, the first metal cation compound and the second metal cation compound are used in the form of a salt solution, and the concentration used is preferably 0.01 mol / L to 0.7 mol / L.

5. The method according to claim 1, characterized in that In step S3, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization temperature is 80°C to 200°C, preferably 120°C to 200°C, and more preferably 130°C to 140°C; the hydrothermal crystallization time is 4h to 96h, preferably 10h to 48h, and more preferably 24h to 36h, and the pressure is autogenous pressure; The conditions of the first calcination treatment include: a calcination temperature of 400°C to 650°C, preferably 500°C to 620°C, and more preferably 550°C to 600°C; and a calcination time of 3h to 12h, preferably 4h to 8h.

6. The method according to claim 1, characterized in that In step S4, the solid-liquid mass volume ratio of the intermediate product to the second metal cation compound used in the form of a solution is 1:(1-200), preferably 1:(5-80); Preferably, the conditions of the second calcination treatment include: a calcination temperature of 400°C to 650°C, preferably 500°C to 620°C, and more preferably 550°C to 600°C; and a calcination time of 3h to 12h, preferably 4h to 8h.

7. The method according to claim 1, characterized in that The step of mixing the intermediate product with the second metal cation compound in step S4 comprises: The intermediate product is dispersed in deionized water, and after heating to 50° C. to 115° C., the second metal cation compound is added, and the pH of the slurry is controlled to be maintained in the range of 7 to 8 using a pH balancing agent, and then the water is removed; Preferably, the pH balancing agent is selected from one or more of ammonia water, n-butylamine, citric acid, lactic acid, ethylenediaminetetraacetic acid and diethyltriaminepentaacetic acid.

8. The clustered ZSM-4 molecular sieve prepared according to the method of any one of claims 1 to 7.

9. A clustered ZSM-4 molecular sieve, characterized in that: The molecular sieve comprises a cluster body, and the cluster body comprises a plurality of nano needle-shaped single crystals.

10. The clustered ZSM-4 molecular sieve according to claim 9, characterized in that: In the cluster, a plurality of nano-needle-shaped single crystals are arranged in parallel; Optionally, the average diameter of the nano needle-shaped single crystals is 50 nm to 80 nm.

11. The clustered ZSM-4 molecular sieve according to claim 9, characterized in that: The total pore volume of the clustered ZSM-4 molecular sieve is 0.001 cm 3 / g~0.7cm 3 / g, preferably 0.01cm 3 / g~0.4cm 3 / g; micropore volume is 0.0005cm 3 / g~0.5cm 3 / g, preferably 0.001cm 3 / g~0.1cm 3 / g; mesopore volume is 0.0005cm 3 / g~0.6cm 3 / g, preferably 0.01cm 3 / g~0.3cm 3 / g; BET specific surface area is 10m 2 / g~400m 2 / g, preferably 60m 2 / g~270m 2 / g; the average pore diameter is 0.56nm to 50nm, preferably 2nm to 20nm.

12. Use of the clustered ZSM-4 molecular sieve according to any one of claims 8 to 11 in the lightening reaction of meta-trimethylbenzene.

13. The use according to claim 12, characterized in that: The reaction conditions of the m-trimethylbenzene lightening reaction include: a temperature of 300°C to 600°C, preferably a temperature of 400°C to 550°C; a pressure of 0.001MPa to 2MPa, preferably a pressure of 0.005MPa to 1MPa, and more preferably a pressure of 0.01MPa to 0.5MPa; a mass space velocity of m-trimethylbenzene of 0.01h -1 ~10h -1 The preferred mass space velocity is 0.05h -1 ~5h -1 , more preferably the mass space velocity is 0.1h -1 ~2h -1 ; Optionally, the meta-trimethylbenzene lightening reaction is carried out under carrier gas conditions, the carrier gas is selected from one or more of the inert gases, the volume flow rate of the carrier gas is 5mL / min to 100mL / min, preferably 10mL / min to 50mL / min, more preferably 10mL / min to 30mL / min; preferably, the inert gas includes N2.

Citation Information

Patent Citations

  • Device for reducing dibenzo-dioxin and dibenzo-furan emissions from catalytic converters containing transition metals

    CN101507900A

  • Method for synthesizing Omega zeolite molecular sieve

    CN112047357A

  • Preparation of omega zeolite

    CN1284475A

  • Faujasite-type zeolite and process for making it

    EP0320114A1

  • Method for making MAZ framework type zeolites

    US20160137519A1