Glass alkali etching process and application thereof
By using sodium hydroxide solution for glass alkali etching, combined with high-temperature stirring and local sandblasting, the safety hazards and environmental pollution problems of the hydrofluoric acid etching process are solved, and the precise thinning of ultra-thin glass and the smooth and translucent surface are achieved , suitable for the manufacture of high-definition displays, and reduces environmental pollution through waste liquid reuse.
Patent Information
- Application Number
- CN202310392590.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-18
AI Technical Summary
The use of hydrofluoric acid in the existing glass etching process has safety hazards and environmental pollution problems, and it is difficult to achieve precise thinning of ultra-thin glass and a smooth and translucent surface, especially when manufacturing high-definition displays, which cannot meet the requirements of low flicker and high definition. needs.
Use 40% to 56% sodium hydroxide solution for glass alkali etching, combined with high-temperature stirring and local sandblasting, control the soaking time and temperature, achieve anti-glare processing and transparent treatment on the glass surface, and remove the white spots after sandblasting The foggy surface simplifies the process and reduces production costs.
It improves the precision and environmental protection of glass etching, reduces environmental pollution, and achieves a smoother, whiter and more translucent anti-glare glass surface. It is suitable for thinning ultra-thin glass and manufacturing high-definition displays, reducing production costs, and Environmental pollution is reduced through the reuse of waste lye.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a glass etching process, in particular to a glass alkali etching process and application thereof. Background Art
[0002] In the field of electronic display screens, common glass processing processes include glass thinning and glass non-refractive light (anti-reflection) processing. Glass thinning mainly uses chemical etching and physical grinding to thin the panel module and display glass to meet the demand for thin and light display products. The following panel application requirements can be achieved by thinning the TFT-LCD panel: 1. Use chemical or physical methods to reduce the thickness of the panel glass to achieve the purpose of thin and light panels; 2. Reduce the weight of the display screen; provide clearer and brighter picture quality; 3. Reduce the occupied space, reduce the thickness of the TFT-LCD module, and leave more space, such as increasing battery capacity; 4. After the glass substrate is thinned, it can achieve a certain degree of flexibility, produce folding or curved screens, and increase better visual effects. The TFT-LCD glass thinning process includes sealing process, etching thinning process and grinding process. The processes for treating the glass surface to eliminate refraction of light (anti-reflection) include etching AG, spraying AG, and coating AG. Among them, etching AG is chemical etching, and the surface is still a glass surface after AG treatment. Since the surface is still glass in nature, the product is not only scratch-resistant, but also has good transmittance and high image clarity. It is recognized by the market as a mainstream anti-glare glass product.
[0003] At present, the mainstream etching technology used in the above-mentioned glass etching thinning process and etching AG process is to use the principle of chemical reaction between hydrofluoric acid chemical solution (HF) and silicon dioxide on the surface of the glass substrate to dissolve it, and then to corrode the panel. As we all know, hydrofluoric acid is highly corrosive, irritating, and contains fluorine hazards. Improper use can cause burns to the human body. Inhalation of high-concentration hydrofluoric acid fumes can cause bronchitis and hemorrhagic pulmonary edema. Hydrofluoric acid fumes can also be absorbed through the skin and cause serious poisoning. Therefore, the acid etching process based on hydrofluoric acid has high requirements for safe ventilation of the etching environment. In addition, improper treatment of hydrofluoric acid waste liquid generated in production will cause serious pollution if it infiltrates into the soil. Excessive discharge of fluorine-containing wastewater will cause major accidents to the water environment. Hydrofluoric acid wastewater is usually neutralized with lime. After the discharge reaches the standard, the stirring flocculation precipitation neutralization process is simple, but it will produce a large amount of hazardous waste containing fluorine lime sludge, which will increase the cost of hazardous waste treatment and the environmental burden. In addition, due to the strong permeability of hydrofluoric acid and mixed acid solution, the etching rate of glass is very fast and the etching time is very short. It is difficult to thin the ultra-thin glass in a short time. It is also difficult to make precise adjustments to the concave and convex shape, haze, gloss, transparency, clarity, D0I (brightness of image), etc. of the glass. It is difficult to manufacture low-flicker glass (Low Sparkle) urgently needed in the field of high-definition display screens such as vehicles, mobile phones, computers, and industrial control. Moreover, the glass surface after acid etching is relatively dark and not clean enough. In view of this, it is necessary to find a safer and more environmentally friendly chemical etching process that can replace acid etching. Summary of the invention
[0004] One of the purposes of the present invention is to provide a glass alkali etching process.
[0005] The technical solution for achieving the first object of the present invention is a glass alkali etching process, wherein the process comprises immersing a glass substrate in an alkali etching solution, wherein the alkali etching solution is a sodium hydroxide solution with a concentration of 40% to 56%, the temperature of the alkali etching solution is 100° C. to 130° C., and the immersion time is 100 min to 300 min.
[0006] Furthermore, the alkali etching solution is stirred during the immersion process to increase the fluidity of the high-temperature liquid in the furnace and the uniformity of the temperature during the immersion process, so that the alkali etching surface is more uniform and transparent, and the height of the concave and convex points is more consistent when it is used for glass anti-glare processing.
[0007] Furthermore, the glass substrate is a glass substrate that has been sandblasted or partially sandblasted or laser engraved or frosted. The glass substrate that has been sandblasted or partially sandblasted is processed by the glass alkali etching process of the present invention to achieve surface anti-glare processing and transparency of the glass.
[0008] Furthermore, the concentration of the sodium hydroxide solution is 46% to 55%. After the sandblasting process, the glass surface is a matte white turbid surface, which affects the transmittance of the glass and the clarity of the display screen, and is easy to produce stains during use and is not easy to wipe. It is necessary to use a glass etching process to remove the foggy white turbidity on the matte surface. On the one hand, the glass should maintain the anti-glare and anti-reflection functions of the matte surface after sand treatment and laser engraving, and on the other hand, the matte spots should be transparent, and the convex spots after sandblasting should be flattened to make the display screen clearer. Alkaline etching can obtain anti-glare glass products with a smoother, flatter, whiter and brighter surface appearance than acid etching.
[0009] Furthermore, the glass substrate after partial sandblasting has a transparent area that does not require anti-glare treatment before sandblasting, and the transparent area is printed with alkali-intolerant protective ink before sandblasting. When the glass substrate enters the alkali etching furnace, the printed protective ink will automatically fall off to form a transparent area, and the glass substrate is etched and de-inked simultaneously using an alkali etching solution, without the need for an additional demolding process, thereby streamlining the process and reducing production costs.
[0010] A second object of the present invention is to provide an application of a glass alkali etching process.
[0011] The technical solution for achieving the second purpose of the present invention is to use the above-mentioned glass alkali etching process to flatten the micro-nano bumps of the anti-glare glass, or to thin the glass substrate below 1 mm, or to thin the glass substrate below 0.2 mm.
[0012] The glass alkali etching process of the present invention can be used for glass thinning and glass surface anti-glare processing. The present invention selects sodium hydroxide (caustic soda) from the industrial "two alkalis" to change the traditional acid etching to alkali etching, thereby improving the etching accuracy of ultra-thin electronic glass and reducing the production cost. In addition, the amount of glass melt (sodium silicate) dissolved in the etching solution in the alkali etching process is not much, and the waste alkali liquid after soaking the glass is cleaner than the alkali waste liquid generated by chemical industries such as textiles, papermaking, and metal materials. The waste alkali liquid generated after the glass alkali etching process can be used as a raw material for wet production of water glass (water glass), and can also be used as an alkaline neutralizer in a sewage treatment plant for secondary reuse. No fluorine-containing wastewater and hazardous fluorine-containing lime sludge are generated during the production process, reducing pollution to the environment, and having a significant environmental protection innovation pollution reduction and emission reduction effect.
[0013] At the same time, the alkali etching process of the present invention is used for the reaction process of sodium hydroxide and glass, which is relatively slow, making the thinning thickness easier to control than acid etching, and is particularly suitable for glass below 1 mm, especially for the thinning of ultra-thin glass below 0.2 mm. On the other hand, when the glass alkali etching process of the present invention is used for the surface anti-glare processing of glass, the sandblasted turbid white layer on the surface of the micro-nano concave-convex pits on the anti-glare frosted glass can be removed during the etching process, making the turbid white layer transparent, improving the clarity and transmittance of the glass, and can also retain tens of millions of transparent micro-nano concave-convex holes by accurately adjusting the alkali solution concentration and the immersion time, so as to retain the diffuse reflection effect, while suppressing the improvement of the intrinsic brightness of the liquid crystal screen, suppressing and controlling the dazzling intrinsic brightness, and obtaining the best DOI value of the display screen. Those skilled in the art can know that the DOI value of the display screen is not the higher the better, but needs to cooperate with the intrinsic brightness of 4K, 5K, 8K high-definition display screens, 4K, 5K, 8K high pixel point changes, easy to write AG concave and convex depth, HZ frequency, find the best balance point between AG diffuse reflected light and intrinsic reflected light, and finally determine the height of the DOI value. The alkali etching process of the present invention reacts slowly and has high adjustment control accuracy, which creates good process conditions for the control and adjustment of the above parameters. The present invention flattens the convex points of micro-nano concave and convex points by precisely adjusting the concentration of alkali etching solution, alkali solution temperature, and immersion time, and realizes the flattening of convex points, reduces the defects of convex points radiating snowflake-shaped flashing points, and realizes the effect of low flicker or no flicker of the screen, and then obtains a smoother, flatter, whiter and more transparent anti-glare glass product than acid etching surface appearance through alkali etching. DETAILED DESCRIPTION Embodiment 1:
[0014] A glass alkali etching process, the process of which includes immersing a glass substrate that has been partially sandblasted in an alkali etching solution, wherein the alkali etching solution is a sodium hydroxide solution with a concentration of 40%, the temperature of the alkali etching solution is 120°C, the immersion time is 300 minutes, and the etching solution is stirred during the immersion process.
[0015] Furthermore, the glass substrate has a transparent area that does not require anti-glare treatment, and the transparent area is printed with alkali-intolerant protective ink.
[0016] Embodiment 2-8 Examples 2-8 adopt the same process as Example 1, except that the process parameters are different, as shown in Table 1. Table 1 also shows the haze value, gloss, distinctness of image and sparkle value of Comparative Examples 1-3 and each embodiment and comparative example, wherein the sparkle value is tested using a flash point tester model SMS-1000.
[0017] Table 1
[0018] As can be seen from Table 1, in Example 1-8, the glass substrates treated by the same sandblasting or partial sandblasting process are alkali-etched using the process parameter range of the present invention. The obtained products have high gloss, low flicker and high transmittance, and can be used to manufacture high-pixel display screens, making the brightness of high-pixel display devices brighter and more uniform, and the naked eye can no longer easily see the flicker of the focus point, which plays an anti-flicker role. In contrast, the products obtained from Comparative Documents 1-3 have low gloss, high flicker value and low clarity, and are unqualified products.
[0019] In the embodiment of the present invention, a non-alkali-resistant protective ink is used to print the transparent area of the glass substrate that does not require anti-glare treatment, and an alkali etching solution is used to simultaneously etch and de-ink the glass substrate, without the need for an additional demolding process, thereby streamlining the process flow and reducing production costs. The glass substrate obtained by the alkali etching process of the present invention can be processed with a dial, a positioning mark, a speaker mesh, a camera hole, etc.
[0020] The present invention also provides an embodiment of using the glass alkali etching process for glass thinning processing, specifically: Example 9
[0021] A glass alkali etching process, the process of which includes immersing a glass substrate in an alkali etching solution, wherein the alkali etching solution is a sodium hydroxide solution with a concentration of 40%, the temperature of the alkali etching solution is 120°C, the immersion time is 300 minutes, and the etching solution is stirred during the immersion process.
[0022] Examples 10-13 Examples 10-13 use the same process as Example 9, except that the process parameters are different, as shown in Table 2. Table 2 also shows the thickness change of the glass substrate before and after alkali etching.
[0023] Table 2
[0024] It can be seen from Examples 9-13 in Table 2 that the alkali etching process of the present invention can be used to replace the traditional acid etching process to perform thinning of the glass substrate within the limited sodium hydroxide solution temperature, immersion temperature and immersion time, thereby meeting the demand for thinning of display products. By adjusting the concentration of the above-mentioned alkali etching solution, the length of time the glass substrate is immersed in the alkali etching solution and the heating temperature of the alkali etching solution can affect the thinning thickness and thinning efficiency of the glass.
[0025] Since the amount of molten glass (sodium silicate) dissolved in the etching solution after the glass is thinned by the alkali etching process is not much, the waste alkali liquid after soaking the glass is cleaner than the alkali waste liquid produced by chemical industries such as textiles, papermaking, and metal materials. The waste alkali liquid produced after the glass alkali etching process can be used as a raw material for the wet production of sodium silicate (water glass), and can also be used as an alkaline neutralizer in a sewage treatment plant for secondary reuse. No fluoride-containing wastewater and hazardous fluoride-containing lime sludge are generated during the production process, which reduces pollution to the environment and has a significant environmental innovation effect of reducing pollution and emissions. If the acid etching process is gradually switched to the alkali etching process in the future, and the waste alkali liquid can be reused to produce sodium silicate, the factory can achieve a waste-free factory, which will have a significant positive ecological impact on protecting the environment and rivers.
[0026] The alkali etching solution of the present invention is a sodium hydroxide solution with a concentration of 40% to 56%. If the concentration of the sodium hydroxide solution is lower than 40%, the immersion time will become slow. If the concentration of the sodium hydroxide solution is higher than the saturation concentration of 56%, there is an operational safety risk. The temperature of the alkali etching solution is adjusted to between 100°C and 130°C. If the temperature is too low, it is difficult to achieve the purpose of thinning. If the glass surface is used for anti-glare processing to remove the white turbid fog on the glass surface, the glass substrate will be immersed in the alkali etching solution for a long time, which will lead to poor appearance of the glass. If the temperature is too high, the alkali solution will boil and rise into the air, which will cause serious production safety problems. Within the concentration and temperature range of the alkali etching solution of the present invention, the etching time cannot exceed 100min to 300min. If the etching time is too short, it will lead to insufficient etching, unqualified product appearance and indicators. If the etching time is too long, the alkali etching solution will excessively erode the product surface, which will also lead to poor product appearance.
[0027] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent process changes made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A glass alkali etching process, characterized in that: The process includes immersing the glass substrate in an alkaline etching solution, wherein the alkaline etching solution is a sodium hydroxide solution with a concentration of 40% to 56%, the temperature of the alkaline etching solution is 100° C. to 130° C., and the immersion time is 100 min to 300 min.
2. The glass alkali etching process according to claim 1, characterized in that: The alkaline etching solution is stirred during the immersion process.
3. The glass alkali etching process according to claim 1, characterized in that: The glass substrate is a glass substrate that has been sandblasted or partially sandblasted or laser engraved or frosted.
4. The glass alkali etching process according to claim 3, characterized in that: The concentration of the sodium hydroxide solution is 46% to 55%.
5. The glass alkali etching process according to claim 3, characterized in that: The glass substrate after partial sandblasting has a transparent area that does not require anti-glare treatment before sandblasting, and the transparent area is printed with alkali-intolerant protective ink before sandblasting.
6. An application of a glass alkali etching process, characterized in that: The glass alkali etching process according to claim 1 is used for thinning a glass substrate with a thickness of less than 1 mm.
7. An application of a glass alkali etching process, characterized in that: The glass alkali etching process according to claim 1 is used for thinning a glass substrate below 0.2 mm.
8. An application of a glass alkali etching process, characterized in that: The glass alkali etching process described in claim 1 is used to level out the micro-nano concave and convex points of the anti-glare glass.
Citation Information
Patent Citations
Glass processing method
CN105693101A
Deinking method for glass workpiece and water-based deinking agent used by deinking method as well as preparation method of water-based deinking agent
CN106398374A
Acid-resisting etching protecting printing ink and its preparation method and construction method
CN107418300A
Methods of reducing the thickness of textured glass, glass-ceramic, and ceramic articles with high concentration alkali hydroxide at elevated temperature