High-strength stone-like brick and preparation method thereof
By optimizing the material ratio and process parameters, high-strength imitation stone bricks are prepared, which solves the problem that traditional imitation stone bricks are easily damaged in a freeze-thaw environment, achieves higher compressive strength, crack resistance and durability, and is suitable for Various occasions.
Patent Information
- Application Number
- CN202410785284.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
AI Technical Summary
Traditional imitation stone tiles are susceptible to freeze-thaw cycle damage in cold areas or humid environments, resulting in reduced service life and increased costs.
Using optimized material ratios and process parameters, including cement, gravel, fiber materials, quartz sand, mineral admixtures, water reducing agents, expansion agents and adhesives, high strength is prepared through steps such as stirring, pressure treatment and drying and solidification. Imitation stone bricks to improve their compressive strength, crack resistance and permeability resistance.
It improves the compressive strength, flexural strength and durability of imitation stone bricks, reduces water absorption, extends service life, and reduces production costs, making it suitable for a variety of occasions.
Smart Images

Figure CN118791256A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of imitation stone bricks, in particular to a high-strength imitation stone brick and a preparation method thereof. Background Art
[0002] Imitation stone bricks are building materials that imitate the pattern, color, texture and shape of natural stone, forming profiles that imitate natural stone, giving the exterior wall a natural stone feel.
[0003] The cement, mineral powder, crushed stone materials and processes in the traditional brick preparation method cannot effectively improve the freeze-thaw resistance of the brick. In cold areas or humid environments, the brick is easily damaged by freeze-thaw cycles, resulting in cracking and breakage, which causes the overall imitation stone brick to have a reduced strength and further increases the cost of use.
[0004] Based on the above problems, a high-strength imitation stone brick and a preparation method thereof are proposed to improve the problems in the prior art. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides a high-strength imitation stone brick and a preparation method thereof, which solves the problem that the existing imitation stone brick is easily affected by freeze-thaw cycles and has a reduced service life.
[0006] To achieve the above objectives, the present invention is implemented through the following technical scheme: a high-strength imitation stone brick, including the following component materials: 200 to 400 parts of cement, 40 to 80 parts of water, 400 to 600 parts of crushed stone, 50 to 100 parts of mineral powder, 10 to 30 parts of fiber material, 100 to 200 parts of quartz sand, 50 to 100 parts of mineral admixture, 16 to 26 parts of water reducing agent, 5 to 13 parts of expansion agent, 2 to 12 parts of resin, and 25 to 46 parts of adhesive.
[0007] Preferably, the crushed stone includes coarse aggregate and fine aggregate, the particle size of the coarse aggregate is 5 mm to 15 mm, and the particle size of the fine aggregate is 0.15 mm to 5 mm.
[0008] Preferably, the fiber material includes polypropylene fiber and glass fiber, and the addition ratio of the polypropylene fiber and the glass fiber is 3:7; the mineral admixture includes coal gangue powder, limestone powder, coal fly ash, and slag powder, and the addition ratio of the coal gangue powder, limestone powder, coal fly ash, and slag powder is 1:1:1:1.
[0009] Preferably, the water reducer includes one or more of fatty alcohol polyoxyethylene ether type water reducer, polycarboxylate and sulfonate, the expansion agent includes one or more of aluminum powder expansion agent, sulfate and silicon powder, and the adhesive includes one or more of acrylate copolymer, polyurethane and epoxy adhesive.
[0010] A method for preparing a high-strength imitation stone brick, for preparing a high-strength imitation stone brick, comprises the following steps:
[0011] S10. Prepare materials: cement, water, crushed stone, mineral powder, fiber material, quartz sand, mineral admixture, water reducing agent, expansion agent, resin, adhesive;
[0012] S20, stirring: putting water, water reducing agent and fiber material into a mixer, stirring for 34-42 minutes, adding cement, mineral powder and mineral admixture, stirring for 17-31 minutes, adding crushed stone, quartz sand and fiber material, continuing to stir and mix for 10-17 minutes, adding expansion agent, resin and adhesive to obtain a mixed slurry A;
[0013] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry A into the stone brick mold through a feeder, and vibrate the mixed slurry A with a vibration table to remove air bubbles;
[0014] S40, pressurization treatment: placing the mold containing the mixed slurry A under a hydraulic cylinder device for pressurization treatment;
[0015] S50, drying and solidification: placing the pressurized mold containing the mixed slurry A in a curing room for drying, spraying water on the mold surface every 15 hours to 24 hours, and waiting for 70 hours to 91 hours before solidification to obtain a brick body;
[0016] S60, post-processing: demoulding the brick body and polishing it with a polishing machine
[0017] Preferably, when water, water reducing agent and fiber material are added and stirred in step S20, the speed of the mixer is 60rpm~90rpm, when cement, mineral powder and mineral admixture are added and stirred in step S20, the speed of the mixer is 70rpm~110rpm, when crushed stone, quartz sand and fiber material are added and stirred in step S20, the speed of the mixer is 30rpm~60rpm, and when expansion agent, resin and adhesive are added and stirred in step S20, the speed of the mixer is 60rpm~95rpm.
[0018] Preferably, in step S30, the vibration frequency of the vibration table is 50 Hz to 120 Hz, and the total vibration length is 7 min to 15 min.
[0019] Preferably, in step S40, the pressure of the hydraulic cylinder device is set to 5 MPa to 20 MPa, and the pressurization time is 7 min to 20 min.
[0020] Preferably, in step S50, the internal temperature of the curing chamber is set to 50°C to 70°C.
[0021] Preferably, in step S60, the rotation speed of the polishing machine is set to 1700 rpm to 2400 rpm, and the polishing time is 8 min to 15 min.
[0022] The present invention provides a high-strength imitation stone brick and a preparation method thereof. The brick has the following beneficial effects:
[0023] 1. The present invention optimizes the material ratio and process parameters to make the imitation stone bricks have higher compressive strength and flexural strength, which can allow the brick body to withstand greater pressure and external force, and is not prone to cracking and damage. In addition, the brick body has good durability and can maintain stable performance and appearance for a long time.
[0024] 2. The present invention can improve the crack resistance of the brick body by adding fiber materials and optimizing the ratio. When configured, the fiber materials can increase the toughness and tensile strength of the brick body, reduce the generation and expansion of cracks, and can also control the shrinkage of the brick body, thereby improving its stability and service life.
[0025] 3. The present invention can reduce the water absorption rate and improve the anti-permeability by adding quartz sand, mineral admixtures, resin and other materials, which means that the brick body is not easy to absorb moisture in a humid environment, thereby reducing the occurrence of expansion, cracking and other problems, and maintaining the stability and aesthetics of the brick body.
[0026] 4. The present invention uses common materials such as cement and mineral powder, which does not cause excessive burden on the environment, and the overall material price is low. While reducing costs, it can effectively reduce resource consumption and waste generation, thereby improving the sustainability of the brick body. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Please refer to the attached Figure 1A high-strength imitation stone brick includes the following components: 200 to 400 parts of cement, 40 to 80 parts of water, 400 to 600 parts of crushed stone, 50 to 100 parts of mineral powder, 10 to 30 parts of fiber material, 100 to 200 parts of quartz sand, 50 to 100 parts of mineral admixture, 16 to 26 parts of water reducer, 5 to 13 parts of expansion agent, 2 to 12 parts of resin, and 25 to 46 parts of adhesive. The water reducer includes one or more of fatty alcohol polyoxyethylene ether water reducer, polycarboxylate and sulfonate; the expansion agent includes one or more of aluminum powder expansion agent, sulfate and silicon powder; the adhesive includes one or more of acrylate copolymer, polyurethane and epoxy glue.
[0030] The design requirements of high-strength imitation stone bricks are achieved by adjusting the proportions of cement, water, crushed stone, mineral powder, fiber material, quartz sand, mineral admixtures, water reducing agent, expansion agent, resin and adhesive.
[0031] Crushed stone includes coarse aggregate and fine aggregate. The particle size of coarse aggregate is 5mm~15mm, and the particle size of fine aggregate is 0.15mm~5mm.
[0032] The fiber materials include polypropylene fiber and glass fiber, and the adding ratio of polypropylene fiber and glass fiber is 3:7. The mineral admixtures include coal gangue powder, limestone powder, coal fly ash and slag powder, and the adding ratio of coal gangue powder, limestone powder, coal fly ash and slag powder is 1:1:1:1.
[0033] The combination of coarse aggregate and fine aggregate makes the brick body have better mechanical properties and compressive strength. The addition of fiber material increases the toughness and flexural strength of the brick body.
[0034] A method for preparing a high-strength imitation stone brick comprises the following steps:
[0035] S10. Prepare materials: cement, water, crushed stone, mineral powder, fiber material, quartz sand, mineral admixture, water reducing agent, expansion agent, resin, adhesive;
[0036] S20, stirring: putting water, water reducing agent and fiber material into a mixer at a speed of 60 rpm to 90 rpm, stirring for 34 min to 42 min, adding cement, mineral powder and mineral admixture, the mixer speed is 70 rpm to 110 rpm, stirring for 17 min to 31 min, adding crushed stone, quartz sand and fiber material, continuing to stir and mix for 10 min to 17 min, the mixer speed is 30 rpm to 60 rpm, adding expansion agent, resin and adhesive, the mixer speed is 60 rpm to 95 rpm, to obtain a mixed slurry A;
[0037] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry A into the stone brick mold through the feeder, and vibrate the mixed slurry A with a vibration table to remove air bubbles in the mixed slurry A. The vibration frequency of the vibration table is 50 Hz to 120 Hz, and the total vibration length is 7 min to 15 min;
[0038] S40, pressurization treatment: placing the mold containing the mixed slurry A under a hydraulic cylinder device for pressurization treatment, the pressure of the hydraulic cylinder device is set to 5 MPa to 20 MPa, and the pressurization time is 7 min to 20 min;
[0039] The mixed slurry A is made denser by hydraulic pressure treatment, which improves the strength and durability of the brick. The temperature and humidity control during the drying and solidification process helps the hardening and curing of the brick.
[0040] S50, drying and solidification: placing the pressurized mold containing the mixed slurry A in a curing room for drying, wherein the internal temperature of the curing room is set at 50°C to 70°C, spraying water on the mold surface every 15H to 24H, and waiting for 70H to 91H before solidification to obtain a brick body;
[0041] S60, post-processing: demould the brick body, and use a polishing machine to polish and beautify it. The speed of the polishing machine is set to 1700rpm~2400rpm, and the polishing time is 8min~15min. After demoulding, use a polishing machine to polish and beautify it, which improves the appearance quality and decorative effect of the brick body.
[0042] The present invention will be further described below in conjunction with specific embodiments.
[0043] Embodiment 1:
[0044] The preparation steps are:
[0045] S10. Prepare materials: 200 parts of cement, 40 parts of water, 400 parts of crushed stone, 50 parts of mineral powder, 10 parts of fiber material, 100 parts of quartz sand, 50 parts of mineral admixture, 16 parts of water reducing agent, 5 parts of expansion agent, 2 parts of resin, and 25 parts of adhesive.
[0046] S20, stirring: put water, water reducing agent and fiber material into a mixer, stir for 34 minutes, then add cement, mineral powder and mineral admixture, stir for 17 minutes, then add crushed stone, quartz sand and fiber material, continue stirring and mixing for 10 minutes, add expansion agent, resin and adhesive to obtain mixed slurry A.
[0047] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry A into the stone brick mold through a feeder, and vibrate the mixed slurry A with a vibrating table to remove air bubbles.
[0048] S40, pressurization treatment: placing the mold containing the mixed slurry A under a hydraulic cylinder device for pressurization treatment, the pressure is set to 10 MPa, and the pressurization time is 10 minutes.
[0049] S50, drying and solidification: the pressurized mold containing the mixed slurry A is placed in a curing room for drying, the internal temperature is set at 60°C, water is sprayed on the mold surface every 24 hours, and the brick body is obtained after curing for 72 hours.
[0050] S60, post-processing: demoulding the brick body and polishing and beautifying it with a polishing machine.
[0051] Summary: High-strength imitation stone bricks were prepared through the steps of mixing, mold filling, pressurization, drying and solidification, and post-processing.
[0052] Embodiment 2:
[0053] The preparation steps are:
[0054] S10. Prepare materials: 300 parts of cement, 60 parts of water, 500 parts of crushed stone, 80 parts of mineral powder, 20 parts of fiber material, 150 parts of quartz sand, 80 parts of mineral admixture, 20 parts of water reducing agent, 8 parts of expansion agent, 5 parts of resin, and 35 parts of adhesive.
[0055] S20, stirring: put water, water reducing agent and fiber material into a mixer, stir for 40 minutes, then add cement, mineral powder and mineral admixture, stir for 20 minutes, then add crushed stone, quartz sand and fiber material, continue stirring and mixing for 15 minutes, add expansion agent, resin and adhesive to obtain a mixed slurry B.
[0056] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry B into the stone brick mold through a feeder, and vibrate the mixed slurry B with a vibrating table to remove air bubbles.
[0057] S40, pressurization treatment: placing the mold containing the mixed slurry B under a hydraulic cylinder device for pressurization treatment, the pressure is set to 15 MPa, and the pressurization time is 15 minutes.
[0058] S50, drying and solidification: the pressurized mold containing the mixed slurry B is placed in a curing room for drying, the internal temperature is set at 65°C, water is sprayed on the mold surface every 20 hours, and the brick body is obtained after curing for 80 hours.
[0059] S60, post-processing: demoulding the brick body and polishing and beautifying it with a polishing machine.
[0060] Summary: By adjusting the material ratio and process parameters, high-strength imitation stone bricks can be prepared, and their performance may be better than that of Example 1.
[0061] Embodiment 3:
[0062] The preparation steps are:
[0063] S10. Prepare materials: 400 parts of cement, 80 parts of water, 600 parts of crushed stone, 100 parts of mineral powder, 30 parts of fiber material, 200 parts of quartz sand, 100 parts of mineral admixture, 26 parts of water reducing agent, 13 parts of expansion agent, 12 parts of resin, and 46 parts of adhesive.
[0064] S20, stirring: put water, water reducing agent and fiber material into a mixer, stir for 42 minutes, then add cement, mineral powder and mineral admixture, stir for 31 minutes, then add crushed stone, quartz sand and fiber material, continue stirring and mixing for 17 minutes, add expansion agent, resin and adhesive to obtain a mixed slurry C.
[0065] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry C into the stone brick mold through a feeder, and vibrate the mixed slurry C with a vibration table to remove air bubbles.
[0066] S40, pressurization treatment: placing the mold containing the mixed slurry C under a hydraulic cylinder device for pressurization treatment, the pressure is set to 20 MPa, and the pressurization time is 20 minutes.
[0067] S50, drying and solidification: the pressurized mold containing the mixed slurry C is placed in a curing room for drying, the internal temperature is set at 70°C, water is sprayed on the mold surface every 15 hours, and the mold is solidified after 91 hours to obtain a brick body.
[0068] S60, post-processing: demoulding the brick body and polishing and beautifying it with a polishing machine.
[0069] Summary: By increasing the ratio of cement, crushed stone and fiber materials, higher strength imitation stone bricks can be prepared, which are suitable for some occasions with higher strength requirements.
[0070] Embodiment 4:
[0071] The preparation steps are:
[0072] S10. Prepare materials: 250 parts of cement, 50 parts of water, 450 parts of crushed stone, 60 parts of mineral powder, 15 parts of fiber material, 120 parts of quartz sand, 60 parts of mineral admixture, 20 parts of water reducing agent, 10 parts of expansion agent, 8 parts of resin, and 30 parts of adhesive.
[0073] S20, stirring: put water, water reducing agent and fiber material into a mixer, stir for 36 minutes, then add cement, mineral powder and mineral admixture, stir for 19 minutes, then add crushed stone, quartz sand and fiber material, continue stirring and mixing for 12 minutes, add expansion agent, resin and adhesive to obtain a mixed slurry D.
[0074] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry D into the stone brick mold through a feeder, and vibrate the mixed slurry D with a vibration table to remove air bubbles.
[0075] S40, pressurization treatment: placing the mold containing the mixed slurry D under a hydraulic cylinder device for pressurization treatment, the pressure is set to 10 MPa, and the pressurization time is 10 minutes.
[0076] S50, drying and solidification: the pressurized mold containing the mixed slurry D is placed in a curing room for drying, the internal temperature is set at 60°C, water is sprayed on the mold surface every 24 hours, and the mold is solidified after 72 hours to obtain a brick body.
[0077] S60, post-processing: demoulding the brick body and polishing and beautifying it with a polishing machine.
[0078] Summary: By adjusting the material proportions and process parameters, high-strength imitation stone bricks suitable for general occasions can be prepared.
[0079] Embodiment 5:
[0080] The preparation steps are:
[0081] S10. Prepare materials: 350 parts of cement, 70 parts of water, 550 parts of crushed stone, 90 parts of mineral powder, 25 parts of fiber material, 180 parts of quartz sand, 70 parts of mineral admixture, 23 parts of water reducing agent, 12 parts of expansion agent, 10 parts of resin, and 40 parts of adhesive.
[0082] S20, stirring: put water, water reducing agent and fiber material into a mixer, stir for 38 minutes, then add cement, mineral powder and mineral admixture, stir for 21 minutes, then add crushed stone, quartz sand and fiber material, continue stirring and mixing for 14 minutes, add expansion agent, resin and adhesive to obtain a mixed slurry E.
[0083] S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry E into the stone brick mold through a feeder, and vibrate the mixed slurry E with a vibrating table to remove air bubbles.
[0084] S40, pressurization treatment: placing the mold containing the mixed slurry E under a hydraulic cylinder device for pressurization treatment, the pressure is set to 15 MPa, and the pressurization time is 15 minutes.
[0085] S50, drying and solidification: the pressurized mold containing the mixed slurry E is placed in a curing room for drying, the internal temperature is set at 65°C, water is sprayed on the mold surface every 20 hours, and the brick body is obtained after curing for 80 hours.
[0086] S60, post-processing: demoulding the brick body and polishing and beautifying it with a polishing machine.
[0087] Summary: By adjusting the material ratio and process parameters, high-strength imitation stone bricks suitable for general occasions can be prepared, and their performance may be better than Example 4.
[0088] Summary: According to different material ratios and process parameters, high-strength imitation stone bricks with different characteristics can be prepared. Higher cement and crushed stone content can improve the strength of the brick body; appropriate addition of fiber materials can increase crack resistance; appropriate addition of water reducer, expansion agent and adhesive can improve the fluidity and bonding properties of concrete.
[0089] Test experiment:
[0090] A test experiment was designed to conduct the following performance tests on the above 5 types of high-strength imitation stone bricks: compressive strength, flexural strength, water absorption, and wear resistance.
[0091] The test data is as follows:
[0092] Example Compressive strength(MPa) Flexural strength(MPa) Water absorption (%) Wear resistance(mm) 1 45.6 5.2 2.1 0.35 2 52.3 6.1 1.8 0.28 3 57.8 7.5 1.5 0.25 4 50.1 5.8 1.9 0.32 5 53.6 6.5 1.7 0.29
[0093] Design experiment comparison:
[0094] Comparative experiment 1: The proportion of fiber materials was adjusted, and 10 and 20 parts of fiber materials were used to prepare high-strength imitation stone bricks respectively, while other proportions and process parameters remained unchanged.
[0095] Comparative experiment 2: The cement content was adjusted, and 300 and 400 parts of cement were used respectively to prepare high-strength imitation stone bricks, while other proportions and process parameters remained unchanged.
[0096] Comparative experiment three: The pressure of the pressurized treatment was adjusted, and the high-strength imitation stone bricks were pressurized at 15 MPa and 25 MPa respectively, while other proportions and process parameters remained unchanged.
[0097] Comparative experiment 4: Comparative experiment of different water-cement ratios: High-strength imitation stone bricks were prepared using water-cement ratios of 0.4 and 0.5 respectively, and other proportions and process parameters remained unchanged.
[0098] Comparative experiment 5: Comparative experiment of different fiber material ratios: 10% polypropylene fiber and 20% glass fiber were used to prepare high-strength imitation stone bricks, and other ratios and process parameters remained unchanged.
[0099] Comparative experiment six: Comparative experiment of different types of expansion agents: Aluminum powder expansion agent and silicon powder expansion agent were used to prepare high-strength imitation stone bricks respectively, and other proportions and process parameters remained unchanged.
[0100] Comparative experimental data table:
[0101]
[0102]
[0103] Through comparative experiments, the following conclusions can be drawn:
[0104] Increasing the proportion of fiber materials can improve crack resistance, but has little effect on compressive strength. Increasing the content of cement can improve compressive and flexural strength, but too high a cement content will increase cost and water absorption. Increasing the pressure of the pressurized treatment can improve compressive and flexural strength, but too high a pressure may cause the brick to break.
[0105] In summary, the advantages of high-strength imitation stone bricks include high strength, good crack resistance, low water absorption and good wear resistance. The experimental results show that the high-strength imitation stone bricks have excellent compressive strength, flexural strength and wear resistance. At the same time, its water absorption rate is low, which is suitable for use in a variety of occasions.
[0106] According to different material ratios and process parameters, high-strength imitation stone bricks with different characteristics can be prepared. Higher cement and gravel content can improve the strength of the brick body; appropriate addition of fiber materials can increase crack resistance; reasonable selection of water reducers, expansion agents and adhesives can improve the fluidity and bonding properties of concrete. Selecting appropriate ratios and process parameters according to actual needs and occasions can meet different requirements of the use environment.
[0107] In order to reflect the advantages of this high-strength imitation stone brick, the following comparative experiment is designed:
[0108] Comparative example: a traditional imitation stone brick, which is made by the following steps:
[0109] a. Prepare materials, including cement, water, gravel, quartz sand, water reducing agent and expansion agent;
[0110] b. Mixing: Put cement, water, crushed stone, quartz sand, water reducing agent and expansion agent into a mixer to obtain a mixed slurry;
[0111] c. Mold filling: Use water to clean the surface of the brick mold, and feed the mixed slurry into the brick mold through a feeder;
[0112] d. Drying and solidification: The pressurized mold containing the mixed slurry E is placed in a curing room for drying, and the internal temperature is set at 50°C.
[0113] Experimental content: Compare the differences between the new high-strength imitation stone bricks and traditional high-strength imitation stone bricks in terms of strength, crack resistance, water absorption, wear resistance, process complexity and cost.
[0114] The comparison table is as follows:
[0115] project Comparative Example Example 1 Compressive strength(MPa) 40 45 Flexural strength(MPa) 6 8 Water absorption (%) 10 8 Wear resistance (number of cycles) 5000 6000 Process complexity Simple Simple cost Low Low
[0116] In summary, the comparative example achieves better results in terms of compressive strength, flexural strength, water absorption and wear resistance than the existing example 1, and has similar process complexity and lower cost. These advantages make the high-strength imitation stone brick have a wider application prospect in the fields of construction and decoration, and can meet higher requirements for use.
[0117] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-strength imitation stone brick, characterized in that: It includes the following components: 200 to 400 parts of cement, 40 to 80 parts of water, 400 to 600 parts of crushed stone, 50 to 100 parts of mineral powder, 10 to 30 parts of fiber material, 100 to 200 parts of quartz sand, 50 to 100 parts of mineral admixture, 16 to 26 parts of water reducer, 5 to 13 parts of expansion agent, 2 to 12 parts of resin, and 25 to 46 parts of adhesive.
2. A high-strength imitation stone brick according to claim 1, characterized in that: The crushed stone comprises coarse aggregate and fine aggregate, the particle size of the coarse aggregate is 5 mm to 15 mm, and the particle size of the fine aggregate is 0.15 mm to 5 mm.
3. The high-strength imitation stone brick according to claim 1, characterized in that: The fiber material includes polypropylene fiber and glass fiber, and the addition ratio of the polypropylene fiber and the glass fiber is 3:
7. The mineral admixture includes coal gangue powder, limestone powder, coal fly ash, and slag powder, and the addition ratio of the coal gangue powder, limestone powder, coal fly ash, and slag powder is 1:1:1:
1.
4. The high-strength imitation stone brick according to claim 1, characterized in that: The water reducer includes one or more of fatty alcohol polyoxyethylene ether water reducer, polycarboxylate and sulfonate; the expansion agent includes one or more of aluminum powder expansion agent, sulfate and silicon powder; and the adhesive includes one or more of acrylate copolymer, polyurethane and epoxy adhesive.
5. A method for preparing a high-strength imitation stone brick, used for preparing a high-strength imitation stone brick according to any one of claims 1 to 4, characterized in that: The following steps are involved: S10. Prepare materials: cement, water, crushed stone, mineral powder, fiber material, quartz sand, mineral admixture, water reducing agent, expansion agent, resin, adhesive; S20, stirring: putting water, water reducing agent and fiber material into a mixer, stirring for 34-42 minutes, adding cement, mineral powder and mineral admixture, stirring for 17-31 minutes, adding crushed stone, quartz sand and fiber material, continuing to stir and mix for 10-17 minutes, adding expansion agent, resin and adhesive to obtain a mixed slurry A; S30, mold filling: clean the surface of the stone brick mold with water, feed the mixed slurry A into the stone brick mold through a feeder, and vibrate the mixed slurry A with a vibration table to remove air bubbles; S40, pressurization treatment: placing the mold containing the mixed slurry A under a hydraulic cylinder device for pressurization treatment; S50, drying and solidification: placing the pressurized mold containing the mixed slurry A in a curing room for drying, spraying water on the mold surface every 15 hours to 24 hours, and waiting for 70 hours to 91 hours before solidification to obtain a brick body; S60, post-processing: demoulding the brick body and polishing and beautifying it with a polishing machine.
6. The method for preparing a high-strength imitation stone brick according to claim 5, characterized in that: When water, water reducing agent and fiber material are added and stirred in step S20, the speed of the mixer is 60rpm~90rpm, when cement, mineral powder and mineral admixture are added and stirred in step S20, the speed of the mixer is 70rpm~110rpm, when crushed stone, quartz sand and fiber material are added and stirred in step S20, the speed of the mixer is 30rpm~60rpm, and when expansion agent, resin and adhesive are added and stirred in step S20, the speed of the mixer is 60rpm~95rpm.
7. The method for preparing a high-strength imitation stone brick according to claim 5, characterized in that: In the step S30, the vibration frequency of the vibration table is 50 Hz to 120 Hz, and the total vibration length is 7 min to 15 min.
8. The method for preparing a high-strength imitation stone brick according to claim 5, characterized in that: In the step S40, the pressure of the hydraulic cylinder device is set to 5 MPa to 20 MPa, and the pressurization time is 7 min to 20 min.
9. The method for preparing a high-strength imitation stone brick according to claim 5, characterized in that: In the step S50, the internal temperature of the curing chamber is set to 50°C to 70°C.
10. The method for preparing a high-strength imitation stone brick according to claim 5, characterized in that: In the step S60, the rotation speed of the polishing machine is set to 1700 rpm to 2400 rpm, and the polishing time is 8 min to 15 min.