Concrete floor repairing material and preparation method thereof
By using combined materials such as mixed cement, aggregate, epoxy resin and polymer materials in concrete floor patching materials, the problem of insufficient compressive strength and bonding force of patching materials in the existing technology is solved, and the repairing effect and use are significantly improved. longevity, achieving more efficient patching and anti-penetration performance.
Patent Information
- Application Number
- CN202410785683.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
AI Technical Summary
The existing concrete floor patching materials have insufficient compressive strength and quick-setting performance, long patching time, poor bonding force, easy falling off and weak anti-penetration ability, and cannot effectively extend the service life of the concrete floor.
Using a combination of mixed cement, mixed aggregate, epoxy resin, polymer materials, concrete sealing curing agent, hardener, adhesion promoter, water reducing agent and air entraining agent, the polymer cement mortar is prepared by stirring to improve the repair material Compressive strength and adhesion, and enhanced anti-penetration capabilities.
It has significantly improved the repair ability and construction efficiency of the concrete floor. The patching material is closely integrated with the concrete floor, has strong anti-penetration ability, extends the service life, and reduces maintenance costs and safety hazards.
Smart Images

Figure CN118791272A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a concrete floor repair material and a preparation method thereof. Background Art
[0002] Concrete is a composite material widely used in civil engineering. It is composed of a variety of basic materials, including cement, sand, stone and water. Concrete floor is a common type of floor, which is mainly formed by pouring, vibrating, leveling and curing of concrete and other raw materials. Concrete floor is widely used in various construction sites such as residential, commercial buildings and industrial facilities because of its economy, simple construction and strong durability.
[0003] Due to structural stress, foundation deformation, temperature changes and other factors, concrete floors will inevitably crack and sand to varying degrees after long-term use. Snow and freeze-thaw will also cause road damage, seriously affecting the performance of the concrete floor. Therefore, it is necessary to regularly repair and control the cracks on the concrete floor to restore the flatness and durability of the concrete floor and extend its service life. The quality of the materials used to repair the concrete floor also directly affects the repair and control effect of the cracks in the concrete floor.
[0004] Most of the existing concrete floor repair materials have a single component, do not have good compressive strength and quick-setting performance, and their comprehensive performance needs to be improved. The ability to repair concrete floor damage is average, and the repair time is also relatively long, which reduces the construction efficiency to a certain extent and cannot effectively avoid the deterioration of the damage problem of the concrete floor. In addition, the repair material is not tightly combined with the concrete floor and is easy to fall off after long-term use. It also does not have good anti-penetration ability and cannot effectively extend the service life of the concrete floor. Therefore, the present invention proposes a concrete floor repair material and a preparation method thereof to solve the problems existing in the prior art. Summary of the invention
[0005] In view of the above problems, the purpose of the present invention is to propose a concrete floor repair material and a preparation method thereof, so as to solve the problems that the comprehensive performance of the existing concrete floor repair materials needs to be improved, the repair ability of the damaged concrete floor is general, the repair time is also relatively long, and the combination of the repair material and the concrete floor is not tight enough, it is easy to fall off after long-term use, and it does not have good anti-penetration ability.
[0006] In order to achieve the purpose of the present invention, the present invention is implemented through the following technical scheme: a concrete floor repair material, comprising the following raw materials in parts by weight: 35-45 parts of mixed cement, 10-15 parts of mixed aggregate, 5-10 parts of epoxy resin, 5-8 parts of polymer material, 3-5 parts of concrete sealing and curing agent, 3-5 parts of hardener, 3-5 parts of adhesion promoter, 1-2.5 parts of water reducer, 0.5-1 part of air entraining agent, and 20-25 parts of water.
[0007] A further improvement is that the mixed cement is prepared by mixing silicate cement and calcium aluminate cement in a mass ratio of 1 to 2:1, and the epoxy resin is selected from one of glycerol epoxy resin and silicone epoxy resin.
[0008] A further improvement is that the mixed aggregate is prepared by mixing coarse aggregate and fine aggregate in a mass ratio of 2 to 3:1, the coarse aggregate is selected from one of slag, crushed stone or ceramsite, and the fine aggregate is selected from one of river sand, mountain sand or machine-made sand.
[0009] A further improvement is that the polymer material is an emulsion polymer, and the emulsion polymer is selected from one of vinyl ester-ethylene copolymer emulsion or acrylic ester emulsion.
[0010] A further improvement is that the concrete sealing curing agent is selected from one of a lithium-based curing agent or a nano-silicon dioxide curing agent, and the hardener is selected from one of a polyurethane-modified hardener or a polyamide-modified hardener.
[0011] A further improvement is that the adhesion promoter is a coupling agent, and the coupling agent is selected from one of a silane coupling agent or a rare earth coupling agent.
[0012] A further improvement is that the water reducer is selected from a naphthalene-based water reducer or an aminosulfonate water reducer, and the air entraining agent is selected from a rosin resin air entraining agent or an alkylbenzene sulfonate air entraining agent.
[0013] A method for preparing a concrete floor repair material comprises the following steps:
[0014] Step 1: first use a measuring scale to weigh 35-45 parts of mixed cement, 10-15 parts of mixed aggregate, 5-10 parts of epoxy resin, 5-8 parts of polymer material, 3-5 parts of concrete sealing curing agent, 3-5 parts of hardener, 3-5 parts of adhesion promoter, 1-2.5 parts of water reducer, 0.5-1 part of air entraining agent and 20-25 parts of water according to the following weight parts, and set aside;
[0015] Step 2: firstly mix and stir the mixed cement, mixed aggregate and water weighed in step 1 to obtain a mixed cement slurry, then sequentially add epoxy resin to the mixed cement slurry and continue to mix and stir to obtain a modified cement slurry, and then add the polymer material to the modified cement slurry and continue to mix and stir to obtain a polymer cement mortar;
[0016] Step 3: First, add the concrete sealing curing agent and adhesion promoter weighed in step 1 into the polymer cement mortar and mix and stir to obtain a mixture, then add the water reducer and air entraining agent into the mixture and continue to mix and stir, and finally add the hardener and stir to obtain a concrete floor repair material.
[0017] A further improvement is that in step 2, the mixed cement, mixed aggregate and water are mixed and stirred for 30 to 40 minutes, the epoxy resin is added to the mixed cement slurry and mixed for 20 to 30 minutes, and the polymer material is added to the modified cement slurry and mixed for 15 to 20 minutes.
[0018] A further improvement is that in step three, the concrete sealing and curing agent and the adhesion promoter are added to the polymer cement mortar and mixed and stirred for 10 to 15 minutes, the water reducer and the air entraining agent are added to the mixture and mixed and stirred for 15 to 20 minutes, and the hardener is added and stirred for another 25 to 30 minutes.
[0019] The beneficial effects of the present invention are as follows: the present invention prepares polymer cement mortar by mixing cement, mixed aggregate, epoxy resin, polymer material and water, so that the subsequently prepared repair material has good compressive strength, and the repair ability of the concrete floor is significantly improved, and it can be applicable to various ground damage defects, and by adding auxiliary materials such as concrete sealing curing agent, hardener, adhesion promoter, water reducer and water reducer, the prepared repair material has good quick-setting performance, and the comprehensive performance is further improved. It can be closely combined with the concrete floor, has good adhesion, is not easy to fall off, and has high anti-penetration ability, which prolongs the service life of the concrete floor to a certain extent, can effectively avoid the deterioration of problems, prevent cracks and potholes from expanding, reduce safety hazards, reduce maintenance costs and frequency, improve the use value of the ground, and meet the use requirements of various places. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1The invention is a schematic flow chart of a method for preparing a concrete floor repair material. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Embodiment 1
[0024] The present embodiment provides a concrete floor repair material, comprising the following raw materials in parts by weight: 35 parts of mixed cement, 15 parts of mixed aggregate, 10 parts of epoxy resin, 5 parts of polymer material, 5 parts of concrete sealing curing agent, 5 parts of hardener, 3 parts of adhesion promoter, 1 part of water reducer, 1 part of air entraining agent, and 20 parts of water, wherein the mixed cement is prepared by mixing silicate cement and calcium aluminate cement in a mass ratio of 1:1, the epoxy resin is glycerol epoxy resin, the mixed aggregate is prepared by mixing coarse aggregate and fine aggregate in a mass ratio of 2:1, wherein the coarse aggregate is slag, the fine aggregate is river sand, the polymer material is an emulsion polymer, the emulsion polymer is a vinyl ester-ethylene copolymer emulsion, the concrete sealing curing agent is a lithium-based curing agent, the hardener is a polyurethane modified hardener, the adhesion promoter is a coupling agent, the coupling agent is a silane coupling agent, the water reducer is a naphthalene-based water reducer, and the air entraining agent is a rosin resin air entraining agent.
[0025] See also Figure 1 This embodiment also provides a method for preparing a concrete floor repair material, comprising the following steps:
[0026] Step 1: First, use a weighing scale to weigh 35 parts of mixed cement, 15 parts of mixed aggregate, 10 parts of epoxy resin, 5 parts of polymer material, 5 parts of concrete sealing curing agent, 5 parts of hardener, 3 parts of adhesion promoter, 1 part of water reducing agent, 1 part of air entraining agent and 20 parts of water according to the following weight parts, and set aside;
[0027] Step 2: First, the mixed cement, mixed aggregate and water weighed in step 1 are mixed and stirred for 30 minutes to obtain a mixed cement slurry, and then the epoxy resin is added to the mixed cement slurry in sequence and the mixture is mixed and stirred for 20 minutes to obtain a modified cement slurry, and then the polymer material is added to the modified cement slurry and the mixture is mixed and stirred for 15 minutes to obtain a polymer cement mortar;
[0028] Step 3: First, add the concrete sealing curing agent and adhesion promoter weighed in step 1 into the polymer cement mortar and mix and stir for 10 minutes to obtain a mixture. Then, add the water reducer and air entraining agent into the mixture and continue mixing and stirring for 15 minutes. Finally, add the hardener and stir for 25 minutes to obtain the concrete floor repair material.
[0029] Embodiment 2
[0030] The present embodiment provides a concrete floor repair material, comprising the following raw materials in parts by weight: 45 parts of mixed cement, 10 parts of mixed aggregate, 5 parts of epoxy resin, 8 parts of polymer material, 3 parts of concrete sealing and curing agent, 3 parts of hardener, 3 parts of adhesion promoter, 2.5 parts of water reducer, 0.5 parts of air entraining agent, and 20 parts of water, wherein the mixed cement is prepared by mixing silicate cement and calcium aluminate cement in a mass ratio of 2:1, the epoxy resin is an organosilicon epoxy resin, the mixed aggregate is prepared by mixing coarse aggregate and fine aggregate in a mass ratio of 3:1, wherein the coarse aggregate is crushed stone, the fine aggregate is mountain sand, the polymer material is an emulsion polymer, the emulsion polymer is an acrylic emulsion, the concrete sealing and curing agent is a nano-silica curing agent, the hardener is a polyamide modified hardener, the adhesion promoter is a coupling agent, the coupling agent is a rare earth coupling agent, the water reducer is an aminosulfonate water reducer, and the air entraining agent is an alkylbenzene sulfonate air entraining agent.
[0031] See also Figure 1 This embodiment also provides a method for preparing a concrete floor repair material, comprising the following steps:
[0032] Step 1: First, use a weighing scale to weigh 45 parts of mixed cement, 10 parts of mixed aggregate, 5 parts of epoxy resin, 8 parts of polymer material, 3 parts of concrete sealing curing agent, 3 parts of hardener, 3 parts of adhesion promoter, 2.5 parts of water reducer, 0.5 parts of air entraining agent and 20 parts of water according to the following weight parts, and set aside;
[0033] Step 2: First, the mixed cement, mixed aggregate and water weighed in step 1 are mixed and stirred for 35 minutes to obtain a mixed cement slurry, and then the epoxy resin is added to the mixed cement slurry in sequence and the mixture is mixed and stirred for 25 minutes to obtain a modified cement slurry, and then the polymer material is added to the modified cement slurry and the mixture is mixed and stirred for 18 minutes to obtain a polymer cement mortar;
[0034] Step 3: First, add the concrete sealing curing agent and adhesion promoter weighed in step 1 into the polymer cement mortar and mix and stir for 12 minutes to obtain a mixture. Then, add the water reducer and air entraining agent into the mixture and continue mixing and stirring for 17 minutes. Finally, add the hardener and stir for 28 minutes to obtain the concrete floor repair material.
[0035] Embodiment 3
[0036] The present embodiment provides a concrete floor repair material, comprising the following raw materials in parts by weight: 38 parts of mixed cement, 12 parts of mixed aggregate, 6 parts of epoxy resin, 6 parts of polymer material, 3 parts of concrete sealing and curing agent, 3 parts of hardener, 5 parts of adhesion promoter, 1.5 parts of water reducer, 0.5 parts of air entraining agent, and 25 parts of water, wherein the mixed cement is prepared by mixing silicate cement and calcium aluminate cement in a mass ratio of 1:1, the epoxy resin is glycerol epoxy resin, the mixed aggregate is prepared by mixing coarse aggregate and fine aggregate in a mass ratio of 2:1, wherein the coarse aggregate is ceramsite, the fine aggregate is machine-made sand (sand obtained by recycling waste concrete), the polymer material is an emulsion polymer, the emulsion polymer is a vinyl ester-ethylene copolymer emulsion, the concrete sealing and curing agent is a lithium-based curing agent, the hardener is a polyurethane modified hardener, the adhesion promoter is a coupling agent, the coupling agent is a rare earth coupling agent, the water reducer is a naphthalene-based water reducer, and the air entraining agent is a rosin resin air entraining agent.
[0037] See also Figure 1 This embodiment also provides a method for preparing a concrete floor repair material, comprising the following steps:
[0038] Step 1: First, use a weighing scale to weigh 38 parts of mixed cement, 12 parts of mixed aggregate, 6 parts of epoxy resin, 6 parts of polymer material, 3 parts of concrete sealing curing agent, 3 parts of hardener, 5 parts of adhesion promoter, 1.5 parts of water reducer, 0.5 parts of air entraining agent and 25 parts of water according to the following weight parts, and set aside;
[0039] Step 2: First, the mixed cement, mixed aggregate and water weighed in step 1 are mixed and stirred for 40 minutes to obtain a mixed cement slurry, and then the epoxy resin is added to the mixed cement slurry in sequence and the mixture is mixed and stirred for 30 minutes to obtain a modified cement slurry, and then the polymer material is added to the modified cement slurry and the mixture is mixed and stirred for 20 minutes to obtain a polymer cement mortar;
[0040] Step 3: First, add the concrete sealing curing agent and adhesion promoter weighed in step 1 into the polymer cement mortar and mix and stir for 15 minutes to obtain a mixture. Then, add the water reducer and air entraining agent into the mixture and continue mixing and stirring for 20 minutes. Finally, add the hardener and stir for 30 minutes to obtain the concrete floor repair material.
[0041] The present invention uses mixed cement, mixed aggregate and water to support mixed cement mortar and uses epoxy resin to mix and modify it, so that the prepared repair material has good compressive strength, adhesion, durability and stability, and can be suitable for various ground damage defects. By mixing the polymer material with the modified cement mortar, the wear resistance and durability of the repair material are further improved, and its repair ability for the concrete floor is significantly improved. By adding a concrete sealing and curing agent, the compressive strength, flexural strength and wear resistance of the repaired concrete floor are improved. By adding an adhesion promoter, the adhesion between the repair material and the concrete floor can be effectively improved, so that it is not easy to fall off. In addition, through the combination of a water reducer and an air entraining agent, the repair material has good anti-penetration ability. Finally, by adding a hardener, the curing speed of the repair material is increased, and the repair construction efficiency of the concrete floor is improved to a certain extent. The preparation process of the entire repair material is simple, easy to operate, and suitable for large-scale production.
[0042] The concrete floor repair materials prepared in Example 1, Example 2 and Example 3 of the present invention were tested and compared with the existing concrete floor repair materials on the market (comparison samples), and the results are shown in Table 1 below:
[0043] Table 1 Test results
[0044]
[0045] It can be seen from Table 1 above that the concrete floor repair materials prepared in Example 1, Example 2 and Example 3 of the present invention are significantly superior to the concrete floor repair materials on the market in terms of early setting, fluidity, compressive strength and water resistance.
[0046] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A concrete floor repair material, characterized in that: The method comprises the following raw materials in parts by weight: 35-45 parts of mixed cement, 10-15 parts of mixed aggregate, 5-10 parts of epoxy resin, 5-8 parts of polymer material, 3-5 parts of concrete sealing and curing agent, 3-5 parts of hardener, 3-5 parts of adhesion promoter, 1-2.5 parts of water reducer, 0.5-1 part of air entraining agent and 20-25 parts of water.
2. A concrete floor repair material according to claim 1, characterized in that: The mixed cement is prepared by mixing silicate cement and calcium aluminate cement in a mass ratio of 1 to 2:1, and the epoxy resin is selected from one of glycerol epoxy resin and silicone epoxy resin.
3. The concrete floor repair material according to claim 1, characterized in that: The mixed aggregate is prepared by mixing coarse aggregate and fine aggregate in a mass ratio of 2 to 3:1, the coarse aggregate is selected from one of slag, crushed stone or ceramsite, and the fine aggregate is selected from one of river sand, mountain sand or machine-made sand.
4. The concrete floor repair material according to claim 1, characterized in that: The polymer material is an emulsion polymer, and the emulsion polymer is selected from one of vinyl ester-ethylene copolymer emulsion or acrylic ester emulsion.
5. The concrete floor repair material according to claim 1, characterized in that: The concrete sealing curing agent is selected from one of a lithium-based curing agent or a nano-silicon dioxide curing agent, and the hardener is selected from one of a polyurethane-modified hardener or a polyamide-modified hardener.
6. The concrete floor repair material according to claim 1, characterized in that: The adhesion promoter is a coupling agent, and the coupling agent is selected from a silane coupling agent or a rare earth coupling agent.
7. The concrete floor repair material according to claim 1, characterized in that: The water reducer is selected from a naphthalene-based water reducer or an aminosulfonate water reducer, and the air entraining agent is selected from a rosin resin air entraining agent or an alkylbenzene sulfonate air entraining agent.
8. A method for preparing a concrete floor repair material as claimed in claim 1, characterized in that: The following steps are involved: Step 1: first use a measuring scale to weigh 35-45 parts of mixed cement, 10-15 parts of mixed aggregate, 5-10 parts of epoxy resin, 5-8 parts of polymer material, 3-5 parts of concrete sealing curing agent, 3-5 parts of hardener, 3-5 parts of adhesion promoter, 1-2.5 parts of water reducer, 0.5-1 part of air entraining agent and 20-25 parts of water according to the following weight parts, and set aside; Step 2: firstly mix and stir the mixed cement, mixed aggregate and water weighed in step 1 to obtain a mixed cement slurry, then sequentially add epoxy resin to the mixed cement slurry and continue to mix and stir to obtain a modified cement slurry, and then add the polymer material to the modified cement slurry and continue to mix and stir to obtain a polymer cement mortar; Step 3: First, add the concrete sealing curing agent and adhesion promoter weighed in step 1 into the polymer cement mortar and mix and stir to obtain a mixture, then add the water reducer and air entraining agent into the mixture and continue to mix and stir, and finally add the hardener and stir to obtain a concrete floor repair material.
9. The method for preparing a concrete floor repair material according to claim 8, characterized in that: In the step 2, the cement, the mixed aggregate and the water are mixed and stirred for 30 to 40 minutes, the epoxy resin is added to the mixed cement slurry and mixed for 20 to 30 minutes, and the polymer material is added to the modified cement slurry and mixed for 15 to 20 minutes.
10. The method for preparing a concrete floor repair material according to claim 8, characterized in that: In the step three, the concrete sealing curing agent and the adhesion promoter are added to the polymer cement mortar and mixed and stirred for 10 to 15 minutes, the water reducing agent and the air entraining agent are added to the mixture and mixed and stirred for 15 to 20 minutes, and the hardener is added and stirred for 25 to 30 minutes.
Citation Information
Patent Citations
Waterproof and anti-corrosion repair mortar for polymer cement-based concrete structure
CN101913827A
Modified cement mortar pavement patching material and pavement patching construction method
CN104591649A
Thin layer repair material for cement concrete pavement
CN108083707A
High-toughness quick-setting repair mortar and preparation method thereof
CN113354374A
Modified cement concrete pavement with high skid resistance and wear resistance and preparation method thereof
CN116496051A