Underwater self-healing photocuring 3D printing elastomer as well as preparation method and application thereof

Through the combination of specific hydrophobic acrylate and fluorine-containing acrylate monomers, combined with photoinitiators and additives, the self-healing ability without special conditions is achieved under room temperature water, which solves the problem of easy breakage of soft robots in underwater environments. problems, improving the application range and repair efficiency of 3D printing elastomers.

CN118791663AActive Publication Date: 2024-10-18SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY

Patent Information

Application Number
CN202410753108.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-18
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Existing 3D printed soft robots are easily damaged in underwater environments and lack self-healing capabilities, making them unable to continue to be used.

Method used

Specific hydrophobic acrylate monomers and fluorine-containing acrylate monomers are used together with photoinitiators and additives to form a photo-cured 3D printing elastomer that can self-heal under water at room temperature. Self-healing is achieved through dipole-dipole interactions. Healing, repair without special conditions.

Benefits of technology

With a repair efficiency of more than 95%, the material can stably self-heal at room temperature and in underwater environments, with an elongation at break greater than 260%, meeting the needs of soft robots for underwater use, and improving light curing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791663A_ABST
    Figure CN118791663A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of 3D printing materials, and discloses an underwater self-healing photocuring 3D printing elastomer as well as a preparation method and application thereof. The photocuring 3D printing elastomer is prepared from the following raw material components: a hydrophobic acrylate monomer, a fluorine-containing acrylate monomer, a photoinitiator and an auxiliary agent, the hydrophobic acrylate monomer is selected from at least one of benzyl acrylate and isobornyl acrylate; the fluorine-containing acrylate monomer is selected from at least one of 2, 2, 2-trifluoroethyl acrylate, and 1H, 1H, 2H, 2H-perfluorooctanol acrylate. On the basis of a polymer network formed by a specific hydrophobic acrylate monomer and a fluorine-containing acrylate monomer, dipole-dipole interaction exists, so that the photocuring 3D printing elastomer can have the self-healing capability under water at room temperature, and the self-healing capability can be realized without stimulation of special conditions (such as heating and laser irradiation).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of 3D printing materials, and in particular relates to an underwater self-healing light-cured 3D printing elastomer and a preparation method and application thereof. Background Art

[0002] The main difference between soft robots and rigid robots is that soft robots are mainly made of soft materials, and their movement is achieved by the deformation of the soft robots themselves. Compared with traditional robots that have poor environmental adaptability and large mass, soft robots have high inherent flexibility, good compliance, excellent adaptability and natural and safe interactivity. This has also made soft robots more and more valued in the fields of medical care, education, service, rescue, exploration, detection, wearable devices, etc., and have shown great development potential.

[0003] At present, the preparation of soft robots mainly relies on mechanical processing, casting and other methods. The steps are cumbersome and time-consuming, and the sealed connection structure needs to occupy a certain space and mass. There are some difficulties in the miniaturization and integrated design of soft robots. Compared with traditional manufacturing methods, 3D printing technology based on digital light processing (DLP) has higher molding accuracy and can quickly build complex three-dimensional structures, which is helpful for the manufacture of soft robots.

[0004] Due to the unique mechanical properties of soft materials, soft robots can adapt to various unstructured environments. However, in practical applications, soft robots usually face complex environments such as underwater operations. Soft materials are very easy to break during use, making them unusable. The emergence of self-healing materials makes it possible for soft robots to continue to be used after being damaged. Compared with traditional materials, self-healing materials show self-repair capabilities when they are broken or fatigued. However, most of the current 3D printed soft robots still rely on commercial elastomers, which do not have the ability to self-heal underwater. Minor defects or puncture wounds can cause devastating damage to soft robots.

[0005] Therefore, providing elastomers that can self-heal underwater at room temperature and can be photocured 3D printed is of great significance to the development of soft robots. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes an underwater self-healing light-cured 3D printed elastomer and its preparation method and application. The light-cured 3D printed elastomer described in the present invention can be photocured and self-healed underwater without special conditions (such as light), and the repair efficiency is above 95%.

[0007] The inventive concept of the present invention: The present invention selects specific hydrophobic acrylate monomers and fluorinated acrylate monomers, and cooperates with photoinitiators and additives, so that the light-cured 3D printing elastomer of the present invention can not only perform efficient light-curing printing, but also based on the polymer network formed by the specific hydrophobic acrylate monomers and fluorinated acrylate monomers, there is a dipole-dipole interaction, so that the light-cured 3D printing elastomer can have self-healing ability under room temperature water, and this self-healing ability can be achieved without the stimulation of special conditions (such as heating, laser irradiation). A stable room temperature self-healing effect can also be maintained in an aqueous environment. The application of light-cured 3D elastomers has been greatly expanded. The elongation at break of the light-cured 3D printing elastomer of the present invention is greater than 260%. After the material is broken, the material can be repaired in a room temperature environment and a room temperature water environment without external stimulation, and the repair efficiency is above 95%.

[0008] In addition, the photocuring efficiency of a single fluorinated acrylate monomer is relatively slow and cannot meet the requirements of 3D printing. The hydrophobic acrylic monomer selected for use in the present invention also helps to improve the photocuring efficiency of the photosensitive resin system.

[0009] A first aspect of the present invention provides an underwater self-healing light-cured 3D printed elastomer.

[0010] Specifically, an underwater self-healing light-curing 3D printing elastomer, the raw material components include a hydrophobic acrylate monomer, a fluorinated acrylate monomer, a photoinitiator, and an auxiliary agent;

[0011] The hydrophobic acrylate monomer is selected from at least one of benzyl acrylate and isobornyl acrylate;

[0012] The fluorine-containing acrylate monomer is selected from at least one of 2,2,2-trifluoroethyl acrylate and 1H,1H,2H,2H-perfluorooctanol acrylate.

[0013] Preferably, the auxiliary agent includes a crosslinking agent and / or a light absorber.

[0014] Preferably, the crosslinking agent is selected from at least one of polyethylene glycol diacrylate, 1,6-hexanediol dimethacrylate, triallyl isocyanurate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol tetraacrylate.

[0015] Preferably, the photoinitiator is selected from at least one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1-hydroxycyclohexyl phenyl ketone.

[0016] Preferably, the light absorber is selected from at least one of Sudan Orange G, Sudan I, quercetin and Marseille Yellow.

[0017] Preferably, the raw material components of the light-cured 3D printing elastomer include 8 to 38 parts of hydrophobic acrylate monomers, 60 to 95 parts of fluorine-containing acrylate monomers, 0.5 to 2.5 parts of photoinitiators, and 0.1 to 1 parts of additives, by weight; further preferably, the raw material components of the light-cured 3D printing elastomer include 10 to 30 parts of hydrophobic acrylate monomers, 70 to 90 parts of fluorine-containing acrylate monomers, 0.5 to 2 parts of photoinitiators, and 0.12 to 0.6 parts of additives, by weight.

[0018] Preferably, the raw material components of the photocurable 3D printing elastomer include 10 to 30 parts of hydrophobic acrylate monomer, 70 to 90 parts of fluorine-containing acrylate monomer, 0.1 to 0.5 parts of crosslinking agent, 0.5 to 2 parts of photoinitiator, and 0.02 to 0.1 parts of light absorber by weight. The appropriate proportion of each component is helpful to obtain a photocurable 3D printing elastomer with better performance.

[0019] A second aspect of the present invention provides a method for preparing an underwater self-healing light-cured 3D printed elastomer.

[0020] Specifically, a method for preparing an underwater self-healing light-cured 3D printed elastomer comprises the following steps:

[0021] The raw material components are mixed and light-cured to obtain the light-cured 3D printed elastomer.

[0022] Preferably, the preparation method comprises the following steps:

[0023] The fluorine-containing acrylate monomer and the hydrophobic acrylate monomer are stirred and mixed, and then a cross-linking agent is added and stirred, and then a photoinitiator and a light absorber are added, stirred and dissolved, and light-cured to obtain the light-cured 3D printing elastomer.

[0024] A third aspect of the present invention provides an application of an underwater self-healing photocurable 3D printed elastomer.

[0025] A soft robot is prepared from the above-mentioned light-cured 3D printed elastomer.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] (1) The present invention selects specific hydrophobic acrylate monomers and fluorinated acrylate monomers, and cooperates with photoinitiators and additives, so that the photocurable 3D printing elastomer of the present invention can not only perform efficient photocuring printing, but also has a dipole-dipole interaction based on the polymer network formed by the specific hydrophobic acrylate monomers and fluorinated acrylate monomers, so that the photocurable 3D printing elastomer can have self-healing ability under room temperature water, and this self-healing ability can be achieved without the stimulation of special conditions (such as heating, laser irradiation). It can also maintain a stable room temperature self-healing effect in a water environment. It greatly expands the application of photocurable 3D elastomers. The elongation at break of the photocurable 3D printing elastomer of the present invention is greater than 260%. After the material is broken, the material can be repaired in a room temperature environment and a room temperature water environment without external stimulation, and the repair efficiency is above 95%.

[0028] (2) The photocurable 3D printed elastomer of the present invention has good stability in an underwater environment and does not require external stimulation. The elastomer can also self-heal in an underwater environment, and its mechanical properties can basically be restored to the initial state.

[0029] (3) The photocurable 3D printed elastomer of the present invention has good stretchability (>260%) and can meet the deformation requirements of soft robots.

[0030] (4) The photocurable 3D printing elastomer of the present invention has a low viscosity raw material photosensitive resin system and can be quickly cured under 405nm or 385nm light. It is suitable for common photocurable 3D printing equipment on the market and has high printing structure accuracy.

[0031] (5) The photocurable 3D printed elastomer of the present invention is highly compatible with DLP 3D printing and can quickly build complex three-dimensional structures with high precision. The pneumatic soft actuator printed with the photocurable elastomer 3D can work stably underwater. After being damaged, the actuator structure can self-heal underwater and continue to work. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The photorheological curves of the photocurable 3D printed elastomers of Example 1 and Comparative Example 1 of the present invention;

[0033] Figure 2 This is a self-healing optical picture of the light-cured 3D printed elastomer in Example 1 of the present invention;

[0034] Figure 3 The self-healing mechanical properties characterization results of the light-cured 3D printed elastomer in Example 1 of the present invention;

[0035] Figure 4The self-healing mechanical properties characterization results of the light-cured 3D printed elastomer under water in Example 1 of the present invention;

[0036] Figure 5 This is an underwater self-healing picture of the 3D printed structure of the light-cured 3D printed elastomer in Example 1 of the present invention;

[0037] Figure 6 This is a self-healing picture of the 3D-printed soft actuator of the photocurable 3D-printed elastomer in water environment in Example 1 of the present invention. DETAILED DESCRIPTION

[0038] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0039] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0040] Example 1: Preparation of photocurable 3D printed elastomer

[0041] The invention discloses an underwater self-healing light-curing 3D printing elastomer. The raw material components are, by weight, 20 parts of isobornyl acrylate, 78.4 parts of 1H,1H,2H,2H-perfluorooctanol acrylate, 0.5 parts of allyl isocyanurate, 1 part of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, and 0.1 parts of Sudan I, a light absorber.

[0042] A method for preparing an underwater self-healing light-cured 3D printed elastomer comprises the following steps:

[0043] 1H,1H,2H,2H-perfluorooctanol acrylate and isobornyl acrylate are stirred and mixed evenly, and then allyl isocyanurate is added and stirred and mixed evenly to obtain a mixed solution; 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and light absorber Sudan I are continued to be added and stirred until completely dissolved to obtain a photosensitive resin liquid; the photosensitive resin liquid is poured into a resin tank of a 3D printing device with a 385nm light source for model printing. After printing is completed, the sample is placed in a UV box and cured for 10 minutes to obtain a light-cured 3D printed elastomer.

[0044] The elongation at break of the light-cured 3D printed elastomer obtained in this embodiment is 270%, and the glass transition temperature is -15°C.

[0045] Comparative Example 1

[0046] This comparative example 1 provides a photocurable resin that does not contain a hydrophobic acrylic monomer, and the preparation method thereof is as follows: take 98.4 parts of 1H,1H,2H,2H-perfluorooctanol acrylate, add 0.5 parts of a cross-linking agent allyl isocyanurate, and stir to mix evenly to obtain a mixed solution; add 1 part of a photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 0.1 parts of a light absorber Sudan I, and stir until completely dissolved to obtain a photocurable resin.

[0047] The photocurable 3D printing elastomer prepared in Example 1 and the photocurable resin without hydrophobic acrylic monomer prepared in Comparative Example 1 were subjected to photorheological characterization, and the entire photocuring process was reflected according to the changes in the storage modulus and loss modulus of the samples, wherein the intersection of the storage modulus and the loss modulus was defined as the gel point, which can be used to quantify the speed of the photocuring process. Figure 1 ("Modulus" represents modulus, and "Time" represents time) as shown in the figure, the photocurable 3D printed elastomer in Example 1 reaches the gel point earlier, and the photocuring speed is significantly improved.

[0048] The self-healing ability of the light-cured 3D printed elastomer prepared in Example 1 was tested.

[0049] Figure 2 This is a self-healing optical picture of the light-cured 3D printed elastomer in Example 1 of the present invention; Figure 2 Before and after healing of light-curing 3D printed elastomers ( Figure 2 The optical microscope picture in which "a" represents before healing and "b" represents after healing shows that after 24 hours of healing, the internal incision of the photocurable 3D printed elastomer completely disappeared, confirming the good self-healing performance of the photocurable 3D printed elastomer.

[0050] Figure 3 The self-healing mechanical properties characterization results of the light-cured 3D printed elastomer in Example 1 of the present invention; Figure 3 It was measured under the conditions that the length of the light-curing 3D printed elastomer spline was 10 mm, the width was 5 mm, the thickness was 1 mm, and the stretching speed was 10 mm / min.

[0051] Depend on Figure 3 (The horizontal axis "Strain" represents the elongation at break, the vertical axis "Stress" represents the fracture strength, and "Original" represents the initial state of the light-cured 3D printed elastomer, that is, the state without cracks) It can be seen that with the extension of the healing time (from 30min to 24h), the elongation at break and the fracture strength of the light-cured 3D printed elastomer gradually recovered. After 24h of healing, the toughness and elongation at break of the light-cured 3D printed elastomer can basically be restored to the initial state.

[0052] Figure 4The self-healing mechanical properties of the light-cured 3D printed elastomer under water are characterized in Example 1 of the present invention; Figure 4 ("Strain" means elongation at break, "Stress" means strength at break, "Original" means the initial state of the photocurable 3D printed elastomer, that is, the state without cracks, and "in water" means in water) It can be seen that after 24 hours of healing in an underwater environment, the strength and elongation at break of the photocurable 3D printed elastomer can basically be restored to the initial state.

[0053] Figure 5 This is an underwater self-healing picture of the 3D printed structure of the light-cured 3D printed elastomer in Example 1 of the present invention; Figure 5 ("a" is a structure 3D printed using the light-curing 3D printed elastomer of Example 1, "b" is two printed structures spliced ​​together in water, "c" is the state of two printed structures being placed underwater for 24 hours after being spliced ​​together, and "d" and "e" are printed structures that can be assembled into a new structure through self-healing splicing after being spliced ​​together, and the interface of the structure will not be destroyed during the stretching process) It can be seen that the light-curing 3D printed elastomer has good 3D printability, and the 3D printed structures can also be assembled into a new structure through self-healing splicing.

[0054] Figure 6 This is a self-healing picture of a 3D-printed soft driver of a light-cured 3D-printed elastomer in a water environment in Example 1 of the present invention; Figure 6 ("a" and "b" are soft drives 3D printed using the light-curing 3D-printed elastomer of Example 1, "c" and "d" are 3D-printed soft drives that can be driven underwater, "e" is a 3D-printed soft drive that cannot be driven after being damaged, and "f" is a 3D-printed soft drive that can continue to be driven after being healed; "Original" represents the initial state of the light-curing 3D-printed elastomer, that is, a state without cracks, "Bending" represents a bent soft drive, "Damaged" represents a damaged soft drive, and "Healed" represents a self-healed soft drive) It can be seen that after the 3D-printed soft drive is damaged, it can self-heal in an aqueous environment and continue to be driven.

[0055] Example 2: Preparation of photocurable 3D printed elastomer

[0056] The invention discloses an underwater self-healing light-curing 3D printing elastomer. The raw material components thereof are, by weight, 30 parts of benzyl acrylate, 68.8 parts of 1H,1H,2H,2H-perfluorooctanol acrylate, 0.1 parts of polyethylene glycol diacrylate, 1 part of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 0.1 parts of Sudan orange as a light absorber.

[0057] A method for preparing an underwater self-healing light-cured 3D printed elastomer comprises the following steps:

[0058] 1H,1H,2H,2H-perfluorooctanol acrylate and benzyl acrylate are stirred and mixed evenly, and then polyethylene glycol diacrylate is added and stirred and mixed evenly to obtain a mixed solution; 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and light absorber Sudan orange are added and stirred until completely dissolved to obtain a photosensitive resin liquid; the photosensitive resin liquid is poured into a resin tank of a 3D printing device with a 385nm light source for model printing. After printing is completed, the sample is placed in a UV box and cured for 10 minutes to obtain a light-cured 3D printed elastomer.

[0059] Example 3: Preparation of photocurable 3D printed elastomer

[0060] The invention discloses an underwater self-healing light-curing 3D printing elastomer. The raw material components are, by weight, 15 parts of isobornyl acrylate, 72.6 parts of 2,2,2-trifluoroethyl acrylate, 0.3 parts of ethoxylated trimethylolpropane triacrylate, 2 parts of 2-hydroxy-2-methyl-1-phenyl-1-propanone, and 0.1 parts of Sudan orange, a light absorber.

[0061] A method for preparing an underwater self-healing light-cured 3D printed elastomer comprises the following steps:

[0062] 2,2,2-trifluoroethyl acrylate and isobornyl acrylate are stirred and mixed evenly, and then ethoxylated trimethylolpropane triacrylate is added and stirred and mixed evenly to obtain a mixed solution; 2-hydroxy-2-methyl-1-phenyl-1-propanone and light absorber Sudan Orange are added and stirred until completely dissolved to obtain a photosensitive resin liquid; the photosensitive resin liquid is poured into a resin tank of a 3D printing device with a 385nm light source for model printing. After printing is completed, the sample is placed in a UV box and cured for 10 minutes to obtain a light-cured 3D printed elastomer.

Claims

1. A light-curing 3D printing elastomer, It is characterized in that The raw material components include hydrophobic acrylate monomer, fluorine-containing acrylate monomer, photoinitiator and auxiliary agent; The hydrophobic acrylate monomer is selected from at least one of benzyl acrylate and isobornyl acrylate; The fluorine-containing acrylate monomer is selected from at least one of 2,2,2-trifluoroethyl acrylate and 1H,1H,2H,2H-perfluorooctanol acrylate.

2. The light-cured 3D printed elastomer according to claim 1, It is characterized in that The auxiliary agent includes a cross-linking agent and / or a light absorber.

3. The light-cured 3D printed elastomer according to claim 1, It is characterized in that The crosslinking agent is selected from at least one of polyethylene glycol diacrylate, 1,6-hexanediol dimethacrylate, triallyl isocyanurate, ethoxylated trimethylolpropane triacrylate, and pentaerythritol tetraacrylate.

4. The light-cured 3D printed elastomer according to claim 1, It is characterized in that The photoinitiator is selected from at least one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1-hydroxycyclohexyl phenyl ketone.

5. The light-cured 3D printed elastomer according to claim 1, It is characterized in that The light absorber is selected from at least one of Sudan Orange G, Sudan I, quercetin and Marseille yellow.

6. The light-cured 3D printed elastomer according to claim 1, It is characterized in that The photocurable 3D printing elastomer comprises, by weight, 8 to 38 parts of hydrophobic acrylate monomers, 60 to 95 parts of fluorine-containing acrylate monomers, 0.5 to 2.5 parts of photoinitiators, and 0.1 to 1 parts of auxiliary agents.

7. The light-cured 3D printed elastomer according to claim 2, It is characterized in that The photocurable 3D printing elastomer comprises, by weight, 10 to 30 parts of hydrophobic acrylate monomers, 70 to 90 parts of fluorine-containing acrylate monomers, 0.1 to 0.5 parts of cross-linking agents, 0.5 to 2 parts of photoinitiators, and 0.02 to 0.1 parts of light absorbers.

8. The method for preparing a light-cured 3D printing elastomer according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The raw material components are mixed and light-cured to obtain the light-cured 3D printed elastomer.

9. The preparation method according to claim 8, It is characterized in that The following steps are involved: The fluorine-containing acrylate monomer and the hydrophobic acrylate monomer are stirred and mixed, and then a cross-linking agent is added and stirred, and then a photoinitiator and a light absorber are added, stirred and dissolved, and light-cured to obtain the light-cured 3D printing elastomer.

10. A soft robot, It is characterized in that Prepared by the light-curing 3D printing elastomer described in any one of claims 1-7.

Citation Information

Patent Citations

  • 3D printing photocuring material and underwater curing after-treatment processing technology thereof

    CN110204661A

  • Multifunctional conductive ionic liquid gel as well as preparation method and application thereof

    CN113549175A

  • Self-healing and 3D printing ionic gel as well as preparation and application thereof

    CN113801272A

  • Underwater self-repairing elastomer based on polymerizable hydrophobic deep-eutectic solvent and synthesis method

    CN114907507A

  • Ultraviolet curing adhesive

    CN115466593A

Cited By

  • Hydrophobic elastomer as well as preparation method and application thereof

    CN119463015A

  • A hydrophobic elastomer and its preparation method and application

    CN119463015B