Environment-friendly stress whitening-resistant ABS (acrylonitrile-butadiene-styrene) resin and preparation method thereof

By adopting the continuous bulk method and grafting reactor technology in the preparation of anti-stress whitening ABS resin, a multi-component copolymer rubber solution with an 'island' structure is formed, which solves the problems of large performance fluctuations and poor environmental protection in the existing technology, and achieves The efficient preparation of environmentally friendly stress-whitening resistant ABS resin improves the material's stress-whitening resistance and recyclability.

CN118791676APending Publication Date: 2024-10-18NORTH HUAJIN CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073455.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing methods for preparing anti-stress whitening ABS resin have large performance fluctuations, high costs, poor environmental protection, and are difficult to recover or recycle.

Method used

The stress-whitening ABS resin is prepared by direct polymerization using a continuous bulk method. The star-shaped branched rubber with low viscosity and low content and the multi-component copolymer rubber solution form an 'island' structure in the grafting reactor to reduce the occurrence of stress concentration and improve Anti-stress whitening performance, and through segmented feeding to accelerate the phase transformation process and improve interface compatibility.

Benefits of technology

It achieves good performance of anti-stress whitening ABS resin, reduces costs, and the product is non-toxic, tasteless, easy to recycle, environmentally friendly, and significantly improves the anti-stress whitening effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981527380000081
    Figure BDA0004981527380000081
  • Figure BDA0004981527380000091
    Figure BDA0004981527380000091
Patent Text Reader

Abstract

The invention relates to the technical field of high-molecular compounds, and particularly discloses environment-friendly stress whitening-resistant ABS (acrylonitrile-butadiene-styrene) resin and a preparation method thereof. The environment-friendly stress whitening-resistant ABS resin is prepared from low-viscosity and low-content rubber through a continuous bulk method, a grafting kettle is additionally arranged in an existing continuous bulk method device, a multipolymer glue solution is added into an original ABS melt, and meanwhile, the ABS glue solution is prepared into the environment-friendly stress whitening-resistant ABS resin in a segmented feeding mode. Compared with the mode of adding the modifier, the ABS resin provided by the invention has excellent stress whitening resistance and is environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer compounds, and specifically discloses an environmentally friendly stress-whitening-resistant ABS resin and a preparation method thereof. Background Art

[0002] High-impact polystyrene, ABS resin, etc., when stretched or bent or damaged by impact, the specimen will turn white. This whitening phenomenon is called stress whitening. When PP, ABS resin and other plastic products are subjected to external forces such as impact, stretching, bending, etc. during manufacturing or use, a large number of microcracks, silver streaks or voids will be generated, resulting in a decrease in the local refractive index of the material, thus showing a white phenomenon. Although stress whitening can improve the impact strength of the material, it will seriously affect the appearance and performance of the product.

[0003] At present, the preparation of stress-whitening ABS resin usually uses high-quality ABS resin as the basic material, and adds appropriate amounts of modifiers, stress-whitening agents and additives. The selection of modifiers is crucial to improving the stress-whitening resistance of ABS resin. Commonly used modifiers include elastomers, rigid particles, etc., which can reduce the occurrence of stress concentration by improving the molecular structure and physical properties of the resin, thereby inhibiting the stress whitening phenomenon. Stress-whitening agents are additives specifically used to improve the stress-whitening resistance of resin materials. It can interact with resin molecules, change the microstructure of the resin, reduce the generation of microcracks and silver streaks, and thus improve the material's stress-whitening resistance. Additives also play an important role in the preparation of stress-whitening ABS resin. They can improve the processing properties of the resin, improve the surface finish of the product, etc., thereby further improving the overall performance of the product.

[0004] Stress-whitening ABS resin is widely used in home appliance housings, auto parts, toys, electronic product housings and other fields. In these fields, products often need to withstand various external forces, such as impact, stretching, etc., so the requirements for stress-whitening resistance are relatively high. The application of stress-whitening ABS resin can effectively improve the appearance quality and performance of products and meet the needs of consumers.

[0005] The existing methods for resisting stress whitening are all modification and blending, but the product performance obtained in this way fluctuates greatly, the cost is increased, and the modified plastic products are difficult to recycle or reuse, or a large amount of pollutants are generated during the recycling process, which greatly reduces the environmental protection.

[0006] As people's requirements for product appearance quality and performance continue to increase, the market demand for stress-whitening ABS resin will continue to grow. In the future, the research and development of stress-whitening ABS resin will pay more attention to improving the comprehensive performance of materials and reducing costs to meet a wider range of application needs. At the same time, with the enhancement of environmental awareness and the popularization of the concept of sustainable development, the research and development of environmentally friendly stress-whitening ABS resin will also become an important direction in the future. Summary of the invention

[0007] The technical problem to be solved by the present invention is: in view of the problems that the existing stress-whitening ABS resin prepared by adding a modifier has large performance fluctuations, high cost and poor environmental protection, a stress-whitening ABS resin is prepared by direct polymerization using a continuous bulk method, which has good environmental protection.

[0008] The technical solution adopted by the present invention is as follows:

[0009] In a first aspect, the present invention provides a method for preparing an environmentally friendly stress-whitening ABS resin, which specifically comprises the following steps:

[0010] S1, 5-10 parts by mass of rubber, 10-20 parts by mass of ethylbenzene, 10-20 parts by mass of acrylonitrile and 60-70 parts by mass of styrene are mixed and dissolved to obtain a uniform raw rubber solution without rubber lumps;

[0011] The rubber is a low-cis star-branched rubber with a 5% rubber styrene solution viscosity between 20 and 80 mPa.s; the star-branched rubber has a three-dimensional shape and a highly branched structure. Compared with linear structure synthetic rubber, the star-branched synthetic rubber has a lower solution viscosity and bulk viscosity, low rubber viscosity, strong system fluidity, easier wrapping of the rubber solution in the reactor and the grafting reactor rubber solution, good interface compatibility between the two, so that the ABS product has the characteristics of faster stress relaxation and insensitivity to shear, and improves the anti-stress whitening effect; low rubber content can further reduce the possibility of stress whitening caused by the presence of dispersed phase in the heterogeneous polymer due to the induction of silver streaks or cracks;

[0012] S2, 10-20 parts by mass of acrylonitrile, 50-60 parts by mass of styrene, 5-10 parts by mass of EPDM rubber, 15-25 parts by mass of ethylbenzene, an initiator, and a chain transfer agent are mixed and dissolved to obtain a grafting glue solution; wherein the amount of the initiator added is 0.01-0.05% of the total mass of the EPDM rubber, acrylonitrile, and styrene, and the amount of the chain transfer agent added is 0.05-0.3% of the total mass of the EPDM rubber, acrylonitrile, and styrene;

[0013] The mass ratio of the original rubber solution obtained in step S1 to the grafted rubber solution obtained in step S2 is 3:1 to 5:1;

[0014] S3, conveying a part of the raw rubber solution of step S1, an initiator, and a chain transfer agent to four plug flow reactors connected in series for continuous bulk polymerization, wherein the polymerization temperature of the first reactor is 103.4-107.4° C., wherein the amount of the initiator added is 0.01-0.05% of the mass sum of the rubber, acrylonitrile, and styrene in the part of the raw rubber solution added, and the amount of the chain transfer agent added is 0.05-0.3% of the mass sum of the rubber, acrylonitrile, and styrene in the part of the raw rubber solution added;

[0015] S4, when the S3 glue solution reacts to the second plug flow reactor, the remaining part of the original glue solution of step S1, the initiator, and the chain transfer agent are transported to the second plug flow reactor, the two glue solutions are mixed and phase transition reaction is carried out in the second reactor at 109.7-117.3°C, and then the melt is continuously transported to the third reactor, wherein the amount of the initiator added is 0.01-0.05% of the mass sum of rubber, acrylonitrile, and styrene in the remaining added part of the original glue solution, and the amount of the chain transfer agent added is 0.05-0.3% of the mass sum of rubber, acrylonitrile, and styrene in the remaining added part of the original glue solution;

[0016] The mass ratio of the original rubber solution added in step S3 to that in step S4 is 1:1 to 19:1;

[0017] S5, when the S4 glue solution reacts to the third plug flow reactor, the S2 grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 120.2-129.4°C, the melt is continuously transported to the fourth reactor;

[0018] S6. After polymerization in the fourth plug flow reactor at 146.6-164.0° C., the material is devolatilized and granulated to prepare an environmentally friendly stress-whitening ABS resin.

[0019] Preferably, the initiator is 1,1-di-tert-butylcyclohexane.

[0020] Furthermore, the amount of 1,1-di-tert-butylcyclohexane added in steps S2 to S4 is 0.03% of the total mass of rubber, acrylonitrile and styrene.

[0021] Preferably, the chain transfer agent is n-dodecyl mercaptan.

[0022] Furthermore, the amount of n-dodecyl mercaptan added in steps S2 to S4 is 0.2% of the total mass of rubber, acrylonitrile and styrene.

[0023] Preferably, in step S6, the devolatilization temperature is 190° C.-240° C., and the vacuum degree is 0.09-0.099 MPa.

[0024] Preferably, in step S1, the amount of rubber added to the original rubber solution is 5wt%.

[0025] Furthermore, the total mass ratio of the grafting liquid to the original rubber liquid is 1:3.

[0026] Furthermore, the raw rubber solution is added into the first and second reactors in stages according to a ratio of 9:1.

[0027] In a second aspect, the present invention provides an environmentally friendly stress-whitening ABS resin, which is prepared by the method described in the first aspect.

[0028] The concept of the present invention is that: on the basis of the continuous bulk method for preparing ABS resin known in the existing industry, a grafting reactor is added between the second reactor and the third reactor. The grafting reactor is a fully mixed reactor. One end of the grafting reactor is connected to the inlet of the third reactor, and the other end is connected to an additional sol tank as the second sol tank. Acrylonitrile, styrene, EPDM rubber and ethylbenzene are added to the sol tank to produce a multi-polymer rubber solution. The rubber solution continues to react with acrylonitrile and styrene in ethylbenzene solvent in the grafting reactor through a chain transfer agent and an initiator to generate a polymerization reaction. The generated ABS grafted rubber solution enters the third reactor and can produce rubber particles with different rubber particle sizes with the ABS melt from the second reactor to form an ABS resin with an "island" structure, which absorbs silver streaks generated by external forces, and slows down or prevents the stress whitening phenomenon of the ABS resin while ensuring the impact performance of the ABS product. The raw rubber liquid is added in stages, that is, 50-95% of the total raw rubber liquid is added to the first reactor, and 5-50% of the total raw rubber liquid is directly added to the second reactor, so that the phase transition can be quickly carried out in the second reactor. The amount of rubber particles embedded in the SAN resin in the ABS generated by the final reaction is lower, the uniformity of the two phases is better, the interface compatibility is better, and the stress whitening phenomenon of ABS is weakened.

[0029] Beneficial effects achieved by the present invention:

[0030] The present invention designs and prepares an environmentally friendly stress-whitening ABS resin. A grafting reactor is added between the second and third reactors of the continuous bulk preparation process known in the industry to prepare a multi-polymer rubber solution and form an "island" structure with the ABS melt in the reactor to absorb silver streaks and avoid stress whitening caused by silver streaks caused by external forces. In addition, low-viscosity and low-content rubber raw materials are used to reduce the content of the dispersed phase, reduce the degree of interface incompatibility, and improve the stress-whitening effect. In addition, segmented feeding is used to accelerate the phase transition speed, reduce the two-phase embedding during the phase transition process, further improve the interface compatibility, and slow down the stress whitening phenomenon. The ABS resin of the present invention not only has a good stress-whitening effect, but also is non-toxic and tasteless, easy to recycle, and environmentally friendly compared to the stress-whitening ABS resin obtained by adding a modifier and blending. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.

[0032] Example 1

[0033] S1: 5%wt rubber, 14wt% ethylbenzene, 16wt% acrylonitrile and 65wt% styrene are mixed and dissolved in a first sol-gel kettle to form a uniform raw rubber solution without rubber lumps, wherein the rubber is Asahi Kasei 720AX;

[0034] S2: dissolving 14% wt acrylonitrile, 58% wt styrene, 8% wt EPDM rubber, 20% wt ethylbenzene, 0.024% initiator 1,1-di-tert-butylcyclohexane, and 0.16% chain transfer agent n-dodecyl mercaptan at 125° C. for 2 hours to prepare a grafting glue solution;

[0035] Wherein m (original glue solution: grafted glue solution = 3:1);

[0036] S3: 50% of the original rubber solution and 0.0129wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.086wt% of the chain transfer agent n-dodecyl mercaptan in the original rubber solution are transported to four plug flow reactors connected in series for continuous bulk polymerization, and the polymerization temperature of the first reactor is 105°C;

[0037] S4, when the S3 glue solution reacts to the second reactor, the remaining 50% of the original glue solution and 0.0129wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.086wt% of the chain transfer agent n-dodecyl mercaptan in the original glue solution are transported to the second reactor, and the two glue solutions are mixed and phase-transition reaction is carried out in the second reactor at 115° C., and then the melt is continuously transported to the third reactor;

[0038] S5, when the S4 glue solution reacts to the third reactor, the grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 125° C., the melt is continuously transported to the fourth reactor;

[0039] S6. The materials polymerized in the fourth reactor at 160.0° C. are devolatilized and granulated at a devolatilization temperature of 220° C. and a vacuum degree of 0.09 MPa to prepare an environmentally friendly stress-whitening ABS resin.

[0040] Example 2

[0041] S1: 10%wt rubber, 14wt% ethylbenzene, 16wt% acrylonitrile and 65wt% styrene are mixed and dissolved in a first sol-gel kettle to form a uniform raw rubber solution without rubber lumps, wherein the rubber is Asahi Kasei 720AX;

[0042] S2: 14% wt acrylonitrile, 58% wt styrene, 8% wt EPDM rubber, 20% wt ethylbenzene, 0.024% initiator 1,1-di-tert-butylcyclohexane, and 0.16% chain transfer agent n-dodecyl mercaptan are dissolved at 125° C. for 2 hours to serve as a grafting glue;

[0043] Wherein m (original glue solution: grafted glue solution = 3:1);

[0044] S3 transports 50% of the original rubber solution and 0.01365wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.091wt% of the chain transfer agent n-dodecyl mercaptan to four plug flow reactors connected in series for continuous bulk polymerization, and the polymerization temperature of the first reactor is 105°C;

[0045] S4, when the S3 glue solution reacts to the second reactor, the remaining 50% of the original glue solution and 0.01365wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.091wt% of the chain transfer agent n-dodecyl mercaptan in the original glue solution are transported to the second reactor, and the two glue solutions are mixed and phase-transition reaction is carried out in the second reactor at 115° C., and then the melt is continuously transported to the third reactor;

[0046] S5, when the S4 glue solution reacts to the third reactor, the grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 125° C., the melt is continuously transported to the fourth reactor;

[0047] S6. The materials polymerized in the fourth reactor at 160.0° C. are devolatilized and granulated at a devolatilization temperature of 220° C. and a vacuum degree of 0.09 MPa to prepare an environmentally friendly stress-whitening ABS resin.

[0048] Example 3

[0049] S1: 5%wt rubber, 14wt% ethylbenzene, 16wt% acrylonitrile and 65wt% styrene are mixed and dissolved in a first sol-gel kettle to form a uniform raw rubber solution without rubber lumps, wherein the rubber is German LANXESS 565T;

[0050] S2: 14% wt acrylonitrile, 58% wt styrene, 8% wt EPDM rubber, 20% wt ethylbenzene, 0.024% initiator 1,1-di-tert-butylcyclohexane, and 0.16% chain transfer agent n-dodecyl mercaptan are dissolved at 125° C. for 2 hours to serve as a grafting glue;

[0051] Wherein m (original glue solution: grafted glue solution = 3:1);

[0052] S3 transports 50% of the original rubber solution and 0.0129wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.086wt% of the chain transfer agent n-dodecyl mercaptan in the original rubber solution to four plug flow reactors connected in series for continuous bulk polymerization, and the polymerization temperature of the first reactor is 105°C;

[0053] S4, when the S3 glue solution reacts to the second reactor, the remaining 50% of the original glue solution and 0.0129wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.086wt% of the chain transfer agent n-dodecyl mercaptan in the original glue solution are transported to the second reactor, and the two glue solutions are mixed and phase-transition reaction is carried out in the second reactor at 115° C., and then the melt is continuously transported to the third reactor;

[0054] S5, when the S4 glue solution reacts to the third reactor, the grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 125° C., the melt is continuously transported to the fourth reactor;

[0055] S6. The materials polymerized in the fourth reactor at 160.0° C. are devolatilized and granulated at a devolatilization temperature of 220° C. and a vacuum degree of 0.09 MPa to prepare an environmentally friendly stress-whitening ABS resin.

[0056] Example 4

[0057] S1: 5%wt rubber, 14wt% ethylbenzene, 16wt% acrylonitrile and 65wt% styrene are mixed and dissolved in a first sol-gel kettle to form a uniform raw rubber solution without rubber lumps, wherein the rubber is Asahi Kasei 720AX;

[0058] S2: 14% wt acrylonitrile, 58% wt styrene, 8% wt EPDM rubber, 20% wt ethylbenzene, 0.024% initiator 1,1-di-tert-butylcyclohexane, and 0.16% chain transfer agent n-dodecyl mercaptan are dissolved at 125° C. for 2 hours to serve as a grafting glue;

[0059] Wherein m (original glue solution: grafted glue solution = 3:1);

[0060] S3 transports 90% of the raw rubber solution and 0.02322wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.1548wt% of the chain transfer agent n-dodecyl mercaptan to four plug flow reactors connected in series for continuous bulk polymerization, and the polymerization temperature of the first reactor is 105°C;

[0061] S4, when the S3 glue solution reacts to the second reactor, the remaining 10% of the original glue solution and 0.00258wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.0172wt% of the chain transfer agent n-dodecyl mercaptan in the original glue solution are transported to the second reactor, and the two glue solutions are mixed and phase-transition reaction is carried out in the second reactor at 115° C., and then the melt is continuously transported to the third reactor;

[0062] S5, when the S4 glue solution reacts to the third reactor, the grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 125° C., the melt is continuously transported to the fourth reactor;

[0063] S6. The materials polymerized in the fourth reactor at 160.0° C. are devolatilized and granulated at a devolatilization temperature of 220° C. and a vacuum degree of 0.09 MPa to prepare an environmentally friendly stress-whitening ABS resin.

[0064] Example 5

[0065] S1: 5%wt rubber, 14wt% ethylbenzene, 16wt% acrylonitrile and 65wt% styrene are mixed and dissolved in a first sol-gel kettle to obtain a uniform raw rubber solution 1 without any rubber lumps, wherein the rubber is Asahi Kasei 720AX;

[0066] S2: 14% wt acrylonitrile, 58% wt styrene, 8% wt EPDM rubber, 20% wt ethylbenzene, 0.024% initiator 1,1-di-tert-butylcyclohexane, and 0.16% chain transfer agent n-dodecyl mercaptan are dissolved at 125° C. for 2 hours to serve as a grafting glue;

[0067] Wherein m (original glue: grafted glue = 5:1);

[0068] S3 transports 50% of the original rubber solution and 0.0129wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.086wt% of the chain transfer agent n-dodecyl mercaptan in the original rubber solution to four plug flow reactors connected in series for continuous bulk polymerization, and the polymerization temperature of the first reactor is 105°C;

[0069] S4, when the S3 glue solution reacts to the second reactor, the remaining 50% of the original glue solution and 0.0129wt% of the initiator 1,1-di-tert-butylcyclohexane and 0.086wt% of the chain transfer agent n-dodecyl mercaptan in the original glue solution are transported to the second reactor, and the two glue solutions are mixed and phase-transition reaction is carried out in the second reactor at 115° C., and then the melt is continuously transported to the third reactor;

[0070] S5, when the S4 glue solution reacts to the third reactor, the grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 125° C., the melt is continuously transported to the fourth reactor;

[0071] S6. The materials polymerized in the fourth reactor at 160.0° C. are devolatilized and granulated at a devolatilization temperature of 220° C. and a vacuum degree of 0.09 MPa to prepare an environmentally friendly stress-whitening ABS resin.

[0072] Test results

[0073] Commercially available ABS8434 was used as a comparative example, and was tested and analyzed together with the ABS resin prepared in Examples 1-6, wherein the melt flow rate: according to the ISO 1133-1-2011 standard method, the test conditions are 220°C, 10kg; stress whitening resistance: the ABS composition was injection molded into a sample with a thickness of 1 mm, a length of 100 mm, and a width of 100 mm, and subjected to a 500g steel ball falling from a height of 50 cm, and the maximum diameter of the whitening area of ​​the sample after the steel ball fell was observed and recorded; the tensile strength was tested according to ISO527 standard, and the cantilever beam notched impact strength was tested according to ISO7619 standard.

[0074] The test results are shown in the following table:

[0075] Table 1 Test results of examples and comparative examples

[0076]

[0077]

[0078] From the above test results, it can be seen that the stress whitening resistance of Examples 1-6 is significantly improved compared with the comparative example, among which Example 4 has the best effect, that is, the rubber addition amount is 5wt%, low viscosity star-branched rubber is used, the mass ratio of grafting kettle glue liquid to original glue liquid is 1:3, and the original glue liquid is added to the first and second reactors in stages according to the ratio of 9:1. The prepared ABS resin has the best two-phase compatibility, faster stress relaxation, the most obvious stress whitening effect, and the impact performance and tensile strength are also at a better level. However, the 565T rubber used in Comparative Example 3 has a higher viscosity, and the stress whitening resistance effect is significantly reduced. Comparative Example 2 uses a large amount of rubber content. Although the impact level is improved, the two-phase compatibility is not good, which will also affect the stress whitening resistance effect. In Comparative Example 5, the amount of multi-copolymer glue liquid added in the grafting kettle is too little, the product has no significant effect on absorbing silver streaks, and the stress whitening resistance is low. Comparative Examples 1 and 4 show that the difference in the amount of original glue liquid added in stages is large, the two-phase embedding amount is reduced, the compatibility is improved, and the corresponding stress whitening resistance effect will be better.

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an environmentally friendly stress-whitening ABS resin, characterized in that: The specific steps include: S1, 5-10 parts by mass of rubber, 10-20 parts by mass of ethylbenzene, 10-20 parts by mass of acrylonitrile and 60-70 parts by mass of styrene are mixed and dissolved to obtain a uniform raw rubber solution without rubber lumps; The rubber is a low-cis star-branched rubber with a 5% rubber styrene solution viscosity between 20 and 80 mPa.s; S2, 10-20 parts by mass of acrylonitrile, 50-60 parts by mass of styrene, 5-10 parts by mass of EPDM rubber, 15-25 parts by mass of ethylbenzene, an initiator, and a chain transfer agent are mixed and dissolved to obtain a grafting glue solution; wherein the amount of the initiator added is 0.01-0.05% of the total mass of the EPDM rubber, acrylonitrile, and styrene, and the amount of the chain transfer agent added is 0.05-0.3% of the total mass of the EPDM rubber, acrylonitrile, and styrene; The mass ratio of the original rubber solution obtained in step S1 to the grafted rubber solution obtained in step S2 is 3:1 to 5:1; S3, conveying a part of the raw rubber solution of step S1, an initiator, and a chain transfer agent to four plug flow reactors connected in series for continuous bulk polymerization, wherein the polymerization temperature of the first reactor is 103.4-107.4° C., wherein the amount of the initiator added is 0.01-0.05% of the mass sum of the rubber, acrylonitrile, and styrene in the part of the raw rubber solution added, and the amount of the chain transfer agent added is 0.05-0.3% of the mass sum of the rubber, acrylonitrile, and styrene in the part of the raw rubber solution added; S4, when the S3 glue solution reacts to the second plug flow reactor, the remaining part of the original glue solution of step S1, the initiator, and the chain transfer agent are transported to the second plug flow reactor, the two glue solutions are mixed and phase transition reaction is carried out in the second reactor at 109.7-117.3°C, and then the melt is continuously transported to the third reactor, wherein the amount of the initiator added is 0.01-0.05% of the mass sum of rubber, acrylonitrile, and styrene in the remaining added part of the original glue solution, and the amount of the chain transfer agent added is 0.05-0.3% of the mass sum of rubber, acrylonitrile, and styrene in the remaining added part of the original glue solution; The mass ratio of the original rubber solution added in step S3 to that in step S4 is 1:1 to 19:1; S5, when the S4 glue solution reacts to the third plug flow reactor, the S2 grafted glue solution is transported to the third reactor, and after the two glue solutions undergo grafting reaction at 120.2-129.4°C, the melt is continuously transported to the fourth reactor; S6. After polymerization in the fourth plug flow reactor at 146.6-164.0° C., the material is devolatilized and granulated to prepare an environmentally friendly stress-whitening ABS resin.

2. The method for preparing the environmentally friendly stress-whitening ABS resin according to claim 1, characterized in that: The initiator is 1,1-di-tert-butylcyclohexane.

3. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 2, characterized in that: The amount of 1,1-di-tert-butylcyclohexane added in steps S2 to S4 is 0.03% of the total mass of rubber, acrylonitrile and styrene.

4. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 1, characterized in that: The chain transfer agent is n-dodecyl mercaptan.

5. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 4, characterized in that: The amount of n-dodecyl mercaptan added in steps S2 to S4 is 0.2% of the total mass of rubber, acrylonitrile and styrene.

6. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 1, characterized in that: In the step S6, the devolatilization temperature is 190° C.-240° C., and the vacuum degree is 0.09-0.099 MPa.

7. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 1, characterized in that: In the step S1, the amount of rubber added to the original rubber solution is 5wt%.

8. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 1, characterized in that: The total mass ratio of the grafting liquid to the original rubber liquid is 1:

3.

9. The method for preparing the environment-friendly stress-whitening ABS resin according to claim 8, characterized in that: The raw rubber solution is added into the first and second reactors in sections according to a mass ratio of 9:

1.

10. An environmentally friendly stress-whitening ABS resin, prepared by the method according to any one of claims 1 to 9.