Method for reducing ash content of polysulfone and polysulfone prepared by same

By using liquid end-capping agent and high-temperature water vapor treatment after the polymerization reaction, the problem of high ash content in polysulfone is solved, polysulfone products with high light transmittance and low haze are achieved, the process flow is simplified and the production cost is reduced. Suitable for industrial production.

CN118791740APending Publication Date: 2024-10-18VONTRON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411105891.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

In the existing polysulfone production process, it is difficult to effectively reduce the ash content of polysulfone, resulting in poor light transmittance and high haze of the product. Moreover, traditional methods consume a large amount of water resources, increase energy consumption, and affect production continuity, safety and reliability.

Method used

After the polymerization reaction is completed, a specific liquid end-capping agent is used to cap the polymer, and high-temperature water vapor is introduced to dissolve the salt impurities and reduce the content of inorganic salts and phenates. Through the salt-forming reaction and polymerization reaction, the polarity Conducted in solvent, reaction conditions and molar ratios were controlled to achieve effective end-capping and work-up.

Benefits of technology

The ash content of the polysulfone resin is significantly reduced, the light transmittance is improved and the haze is reduced. The process is simple, the cost is low, it is suitable for industrial production, and it is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118791740A_ABST
    Figure CN118791740A_ABST
Patent Text Reader

Abstract

The invention relates to a method for reducing ash content of polysulfone and polysulfone prepared by the method. The method comprises the following steps: adding an aromatic diphenol monomer, a dihalogenated diphenyl sulfone monomer and a catalyst into a polar solvent for salt forming reaction and polymerization reaction, wherein the catalyst is one or more of sodium and potassium hydroxides, carbonate and bicarbonate; the method comprises the following steps of: adding an end-capping reagent to carry out an end-capping reaction after the viscosity of a reaction system reaches 8000-75000 mPa.s, introducing water vapor at the temperature of more than or equal to 100 DEG C, and the end-capping reagent is one or more of compounds with the following structural formula: # imgabs0 #, and the molar ratio of the end-capping reagent to the aromatic diphenol monomer is (0.003-0.05): 1. According to the method disclosed by the invention, the ash content of the polysulfone resin can be obviously reduced, and the obtained polysulfone product has high light transmission, low haze and low monomer content. The method disclosed by the invention is simple in process, low in manufacturing cost and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for reducing the ash content of polysulfone and polysulfone prepared by the method, belonging to the technical field of reducing the ash content of polysulfone. Background Art

[0002] Polysulfone is a kind of thermoplastic engineering plastic that appeared in the mid-to-late 1960s. It is a slightly amber, amorphous, transparent or translucent polymer with sulfone groups and aromatic nuclei on the main chain of the molecule. Polysulfone has excellent mechanical properties, good rigidity and toughness, wear resistance, corrosion resistance to inorganic acids, alkalis, and salt solutions, resistance to ion radiation, easy molding and processing, and can maintain excellent mechanical properties even at high temperatures. It is used in many fields such as water treatment, aerospace, automobiles, tableware, and medical equipment.

[0003] The industrial production of polysulfone mostly adopts a one-step process. The one-step process is divided into a polymerization stage and a post-processing stage. The polymerization stage mainly reacts bisphenol A, 4,4'-dichlorodiphenyl sulfone (or 4,4'-difluorodiphenyl sulfone), and potassium carbonate (or potassium hydroxide, sodium hydroxide, sodium carbonate, etc.) in an organic solvent. The post-processing stage uses a solvent different from the previous polymerization process as a precipitant, and injects the polymerized viscous liquid into it. At this time, polysulfone will be separated from the polymer solution, and then purified, dried, granulated and packaged.

[0004] The separation and purification steps of polysulfone from polymer solution are particularly important, as they affect various properties of polysulfone. The polymer solution after polymerization contains unreacted inorganic salts such as carbonates or bicarbonates, reaction byproducts such as halides such as potassium chloride, unreacted phenol salts, coloring metal ions brought by the system and materials, and other mechanical impurities. These impurities are difficult to remove, resulting in the ash content of most products being above 0.2%. Problems caused by high ash content include, for example: defects are easily generated on the surface of the separation membrane produced; the polysulfone injection molded parts produced have poor light transmittance and high haze; when used in the field of hemodialysis, the ash impurities therein will precipitate, thus affecting its application in high-end industries, etc.

[0005] In the current polysulfone industrial production method, the main processes for reducing ash content include the following categories:

[0006] Multiple water washing or hot water washing, such as CN 110128656 B, CN 110272545 B, CN 103613752A, CN102690412 A, CN 102888003 A, the defects of this method are: multiple water washing requires a lot of water resources, resulting in waste of water resources, higher post-processing costs, and increased time costs. Hot water washing will increase more energy consumption, and this method has limited ash removal effect.

[0007] Precipitate or wash in solvents other than water, such as CN 101693764 B, CN 113999394A, CN115850704 A, CN 115785446 A, CN 116178719 A, CN 115926167A, CN 103897188 B. The defects of this method are: using methanol, ethanol, acetone, acetonitrile, etc. as precipitation solvents or washing solvents, this method is slightly better than using only water to remove ash, but the problem brought about by this is that the components in the waste liquid increase, which increases the difficulty of waste liquid recovery and treatment, and the introduction of volatile organic solvents reduces the safety and reliability of production.

[0008] After the polymerization is completed, centrifugation or static sedimentation is performed, and the upper clear liquid is taken for post-processing, such as CN 104629055 B, CN108329472A, and CN 107286345B. The disadvantages of this method are that no matter centrifugation or static sedimentation, it will affect the production continuity and reduce the production efficiency. At the same time, the salt-rich solution in the lower layer is also difficult to process.

[0009] After the polymerization, a surfactant is added to the solution or the powder after crushing for cleaning, such as CN114561013B and CN 111303427A. The disadvantages of this method are that a third (or even more) impurities are introduced, and the surfactant cannot be completely removed in the subsequent treatment. At the same time, most surfactants are not resistant to high temperatures and will decompose during subsequent granulation or other high-temperature treatments, thereby reducing the performance of polysulfone. Summary of the invention

[0010] Problem that the invention aims to solve

[0011] The object of the present invention is to solve the above-mentioned problems existing in the existing technology for removing ash from polysulfone.

[0012] Solutions for solving problems

[0013] In order to achieve the above-mentioned purpose, the inventors conducted in-depth research and unexpectedly found that after the polymerization reaction is completed, the obtained polymer is capped with a specific liquid capping agent to reduce the amount of phenolate at the molecular chain end of the polysulfone and then high-temperature water vapor is introduced into the polymer solution to dissolve the salt impurities therein, which can greatly reduce the unreacted inorganic salts such as carbonates or bicarbonates, monomer reactants, reaction by-products such as halides such as potassium chloride, unreacted phenolate, coloring metal ions and other mechanical impurities brought by the system and materials in the polysulfone product, thereby improving the quality of the polysulfone product.

[0014] The present invention provides a method for reducing the ash content of polysulfone, which comprises:

[0015] Adding aromatic diphenol monomers, dihalogenated diphenyl sulfone monomers and catalysts into a polar solvent to carry out salt-forming reaction and polymerization reaction, wherein the catalyst is one or more of sodium and potassium hydroxides, carbonates and bicarbonates;

[0016] After the viscosity of the reaction system reaches 8000-75000 mPa·s, a capping agent is added to carry out a capping reaction, and then water vapor is introduced, wherein the water vapor temperature is ≥100° C., and the capping agent is one or more compounds having the following structural formula:

[0017]

[0018] The molar ratio of the end-capping agent to the aromatic diphenol monomer is (0.003-0.05):1;

[0019] The obtained polymer solution is post-treated.

[0020] In the method of the present invention, the dihalogenated diphenyl sulfone monomer is at least one of 4,4'-dichlorodiphenyl sulfone and 4,4'-difluorodiphenyl sulfone, and the aromatic diphenol monomer is bisphenol A.

[0021] The method of the present invention, wherein the molar ratio of the aromatic diphenol monomer to the dihalogenated diphenyl sulfone monomer is 1: (1.001-1.04); the molar ratio of the catalyst to the aromatic diphenol monomer is (1.05-1.45):1.

[0022] In the method of the present invention, the polar solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and sulfolane.

[0023] In the method of the present invention, the amount of the polar solvent added is 1 to 4 times the total mass of the aromatic diphenol monomer, the dihalogenated diphenyl sulfone monomer and the catalyst.

[0024] The method of the present invention, wherein the post-treatment comprises precipitating the polymer solution in water.

[0025] The present invention also provides a polysulfone obtained by the method of the present invention.

[0026] Effects of the Invention

[0027] By using the method of the present invention, the ash content in the polysulfone resin can be greatly reduced from about 500ppm in the traditional method to below 35ppm, and the product obtained by injection molding the polysulfone resin obtained by the method has the advantages of high light transmittance, low haze and low monomer content. The method of the present invention has simple process, low manufacturing cost, no need to modify existing equipment, is suitable for industrial production, and is environmentally friendly. DETAILED DESCRIPTION

[0028] Various exemplary embodiments, features and aspects of the present invention will be described in detail below. The word "exemplary" used here means "used as an example, embodiment or illustrative". Any embodiment described here as "exemplary" is not necessarily interpreted as being superior or better than other embodiments.

[0029] In addition, in order to better illustrate the present invention, numerous specific details are provided in the following specific embodiments. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In other examples, methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the subject matter of the present invention.

[0030] Unless otherwise stated, the units used in this specification are all international standard units, and the numerical values ​​and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.

[0031] In this specification, the word "may" means both performing a certain process and not performing a certain process.

[0032] In this specification, the references to "some specific / preferred embodiments", "other specific / preferred embodiments", "embodiments", etc., mean that the specific elements (e.g., features, structures, properties and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not exist in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0033] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints numerical values ​​A and B.

[0034] The present invention provides a method for reducing the ash content of polysulfone, which comprises:

[0035] Adding aromatic diphenol monomers, dihalogenated diphenyl sulfone monomers and catalysts into a polar solvent to carry out salt-forming reaction and polymerization reaction, wherein the catalyst is one or more of sodium and potassium hydroxides, carbonates and bicarbonates;

[0036] After the viscosity of the reaction system reaches 8000-75000 mPa·s, a capping agent is added to carry out a capping reaction, and then water vapor is introduced, wherein the water vapor temperature is ≥100° C., and the capping agent is one or more compounds having the following structural formula:

[0037]

[0038] The molar ratio of the end-capping agent to the aromatic diphenol monomer is (0.003-0.05):1;

[0039] The obtained polymer solution is post-treated.

[0040] At present, the industrial production of polysulfone usually uses methyl chloride for end-capping, but gaseous methyl chloride is not easy to be evenly dispersed in a high-viscosity polymer solution to carry out an effective end-capping reaction. The specific end-capping agent used in the present invention is in a liquid state after entering the reactor, and can be more evenly dispersed than methyl chloride, so the end-capping effect is also better. Better end-capping will reduce the amount of phenolate at the molecular chain end of the polysulfone resin finally obtained, thereby reducing the ash content, and at the same time, due to the reduction of the content of phenolate at the molecular chain end, the degree of color change of the resin during subsequent high-temperature processing is reduced.

[0041] In addition, after the end-capping is completed, high-temperature water vapor is continuously introduced into the polymer solution to dissolve unreacted inorganic salts such as carbonates or bicarbonates, monomer reactants, reaction by-products such as halides such as potassium chloride, unreacted phenol salts, soluble impurities in the system, etc. Since water and solvents are miscible, water vapor can be well dispersed in the polymer solution and quickly dissolve impurities such as salts.

[0042] The method of the present invention can avoid the phenomenon of large-scale precipitation, agglomeration, and caking of polysulfone caused by the local appearance of a large amount of liquid water in the polymer solution when liquid water is directly added. The agglomerated or caked polysulfone will contain impurities such as salts, and these contained salts will be difficult to remove later.

[0043] When the molar ratio of the end-capping agent to the aromatic diphenol monomer is (0.003-0.05):1, effective end-capping can be achieved without excess end-capping agent. If the molar ratio is lower than 0.003:1, effective end-capping cannot be achieved. If the molar ratio is higher than 0.05:1, impurities are introduced due to excess end-capping agent.

[0044] Preferably, the molar ratio of the end-capping agent to the aromatic diphenol monomer is (0.008-0.01):1.

[0045] Preferably, the aromatic diphenol monomer is bisphenol A.

[0046] Preferably, the dihalogenated diphenyl sulfone monomer is at least one of 4,4′-dichlorodiphenyl sulfone and 4,4′-difluorodiphenyl sulfone.

[0047] Preferably, the molar ratio of the aromatic diphenol monomer to the dihalogenated diphenyl sulfone monomer is 1:(1.001-1.04).

[0048] Preferably, the molar ratio of the catalyst to the aromatic diphenol monomer is (1.05-1.45):1.

[0049] When the molar ratio of the catalyst to the aromatic diphenol monomer is (1.05-1.45):1, the catalytic reaction can be carried out quickly. If the molar ratio is lower than the lower limit, the reaction rate is greatly slowed down. If the molar ratio is higher than the upper limit, it will lead to problems such as difficulty in handling the excess solid catalyst and increased costs.

[0050] Preferably, the molar ratio of the catalyst to the aromatic diphenol monomer is (1.1-1.25):1.

[0051] Preferably, the polar solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and sulfolane.

[0052] Preferably, the amount of the polar solvent added is 1 to 4 times the total mass of the aromatic diphenol monomer, the dihalogenated diphenyl sulfone monomer, and the catalyst. If it is less than 1 time, it is not conducive to uniform mixing of the reactants, thereby affecting the reaction. If it is more than 4 times, the excess solvent is difficult to post-process, and the cost is increased.

[0053] Preferably, the post-treatment comprises precipitating the polymer solution in water.

[0054] More preferably, the polysulfone precipitated in water is pulverized, washed with water, dried, and granulated.

[0055] Preferably, the salt-forming reaction is carried out at a temperature ranging from 130 to 160°C, and the polymerization reaction is carried out at a temperature ranging from 190 to 230°C.

[0056] Preferably, the salt-forming reaction and the polymerization reaction are carried out for 5 to 15 hours, the end-capping reaction is carried out for 0.5 to 3 hours, and the water vapor introduction time is continued for 0.5 to 3 hours; more preferably, the oxygen content in the water vapor is ≤0.01%.

[0057] Preferably, after adding the aromatic diphenol monomer, the dihalogenated diphenyl sulfone monomer, the catalyst and the polar solvent, the air in the reaction kettle is replaced by vacuuming and filling with nitrogen. More preferably, the replacement frequency is 5 to 10 times.

[0058] Example

[0059] The embodiments of the present invention will be described in detail below in conjunction with the examples, but those skilled in the art will appreciate that the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. If no specific conditions are specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0060] The structure of end-capping agent A is as follows:

[0061]

[0062] The structure of the end-capping agent B is as follows:

[0063]

[0064] The structure of the capping agent C is as follows:

[0065]

[0066] The structure of the end-capping agent D is as follows:

[0067]

[0068] Example 1

[0069] 500g of bisphenol A, 631g of 4,4′-dichlorodiphenyl sulfone and 363g of potassium carbonate were added to 2820g of N,N-dimethylacetamide in sequence. After nitrogen substitution, the temperature was raised to 145°C and maintained for 4h to complete the salt-forming reaction. After the salt-forming reaction was completed, the temperature was raised to 195°C and maintained for 8h to complete the polymerization reaction. After the system reached the target viscosity of 50000mPa·s, 0.9g of end-capping agent A was immediately added for end-capping reaction. After reacting for 2h, high-temperature water vapor (100°C) was introduced to maintain the pressure in the autoclave at 0.05MPa. After continuous introduction for 1.5h, the polymer solution was precipitated in water, crushed, washed, centrifuged, dried and granulated.

[0070] Example 2

[0071] Example 2 was carried out in the same manner as Example 1, except that 2.65 g of the end-capping agent A was added.

[0072] Example 3

[0073] Example 3 was carried out in the same manner as Example 1, except that 15 g of the end-capping agent A was added.

[0074] Example 4

[0075] Example 4 was carried out in the same manner as Example 1 except that 2.3 g of the capping agent B was added.

[0076] Example 5

[0077] Example 5 was carried out in the same manner as Example 1 except that 2.65 g of the capping agent C was added.

[0078] Example 6

[0079] Example 6 was carried out in the same manner as Example 1, except that 3.96 g of the capping agent D was added.

[0080] Example 7

[0081] Example 7 was carried out in the same manner as Example 2, except that the high-temperature steam was continuously introduced for 0.5 h.

[0082] Example 8

[0083] Example 8 was carried out in the same manner as Example 2, except that the high-temperature steam was continuously introduced for 2.5 h.

[0084] Example 9

[0085] Example 9 was carried out in the same manner as Example 2, except that the high-temperature steam was continuously introduced for 3 hours.

[0086] Comparative Example 1

[0087] 500g of bisphenol A, 631g of 4,4′-dichlorodiphenyl sulfone and 363g of potassium carbonate were added to 2800g of N,N-dimethylacetamide in sequence. After nitrogen substitution, the temperature was raised to 145°C and maintained for 4 hours to complete the salt-forming reaction. After the salt-forming reaction was completed, the temperature was raised to 195°C and maintained for 8 hours to complete the polymerization reaction. After the system reached the target viscosity of 50000mPa·s, methyl chloride was introduced for end-capping for 1 hour, and then the polymer solution was precipitated in water, crushed, washed, centrifuged, dried and granulated.

[0088] Comparative Example 2

[0089] Comparative Example 2 was carried out in the same manner as Comparative Example 1 except that methyl chloride was introduced for 3 h for end-capping.

[0090] Performance Testing

[0091] The performance tests were carried out on the samples of the above embodiments and comparative examples, and the results are listed in the following Table 1.

[0092] Table 1

[0093]

[0094] Turbidity 1 is the result of taking the granulated samples of the polysulfone resin of each embodiment and comparative example and dissolving them in DMF (the mass fraction of the sample is 20%), and then standing to cool to room temperature (25±3°C) and testing immediately, and turbidity 2 is the result of standing to stand for 10 days. The ash content test is carried out in accordance with GB / T 9345-2008, the light transmittance and haze are carried out in accordance with GB / T 2410-2008, and the total migration amount is carried out in accordance with GB 31604.8-2023 (the "total migration amount" tests the residual amount of impurities including monomers in the product).

[0095] By comparing the results of Examples 1-9 and Comparative Examples 1-2, it can be seen that by capping the polysulfone with a specific capping agent and passing high-temperature water vapor, the turbidity, ash content and residual impurity content can be significantly reduced. Therefore, the light transmittance of the obtained polysulfone is improved and the haze is reduced.

[0096] It should be noted that, although the technical solution of the present invention is introduced with specific examples, those skilled in the art will appreciate that the present invention should not be limited thereto.

[0097] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or technical improvements in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A method for reducing the ash content of polysulfone, comprising: Adding aromatic diphenol monomers, dihalogenated diphenyl sulfone monomers and catalysts into a polar solvent to carry out salt-forming reaction and polymerization reaction, wherein the catalyst is one or more of sodium and potassium hydroxides, carbonates and bicarbonates; After the viscosity of the reaction system reaches 8000-75000 mPa·s, a capping agent is added to carry out a capping reaction, and then water vapor is introduced, wherein the water vapor temperature is ≥100° C., and the capping agent is one or more compounds having the following structural formula: The molar ratio of the end-capping agent to the aromatic diphenol monomer is (0.003-0.05):1; The obtained polymer solution is post-treated. 2 . The method according to claim 1 , wherein the dihalogenated diphenyl sulfone monomer is at least one of 4,4′-dichlorodiphenyl sulfone and 4,4′-difluorodiphenyl sulfone, and the aromatic diphenol monomer is bisphenol A.

3. The method according to claim 1 or 2, wherein the molar ratio of the aromatic diphenol monomer to the dihalogenated diphenyl sulfone monomer is 1:(1.001-1.04); the molar ratio of the catalyst to the aromatic diphenol monomer is (1.05-1.45):

1.

4. The method according to claim 1 or 2, wherein the polar solvent is at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and sulfolane.

5. The method according to claim 1 or 2, wherein the amount of the polar solvent added is 1 to 4 times the total mass of the aromatic diphenol monomer, the dihalogenated diphenyl sulfone monomer, and the catalyst.

6. The method according to claim 1 or 2, wherein the post-treatment comprises precipitating the polymer solution in water. 7 . Polysulfone obtained by the method according to claim 1 .