Ultraviolet-proof polymer composite material and preparation method thereof
Through the combination of modified polyethylene terephthalate and nanoparticle ZnO and modification with silane coupling agent, the problems of shortened service life of polymer composite materials under ultraviolet light and uneven mixing of raw materials are solved, and efficient UV absorption and improved mechanical properties.
Patent Information
- Application Number
- CN202411077330.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-18
AI Technical Summary
The service life of existing polymer composite materials is shortened under ultraviolet irradiation, and uneven mixing of raw materials during the preparation process leads to insufficient performance.
Modified polyethylene terephthalate is combined with modified ZnO nanoparticles, and modified through grafting reaction and silane coupling agent to form a polymer composite material with good ultraviolet absorption and dispersion.
The UV resistance and mechanical properties of composite materials are improved, the service life is extended, and the raw materials are evenly dispersed and firmly combined.
Smart Images

Figure BDA0004982709060000101 
Figure BDA0004982709060000102 
Figure BDA0004982709060000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an ultraviolet-proof polymer composite material and a preparation method thereof. Background Art
[0002] Ultraviolet rays are electromagnetic waves with a wavelength of 180-400nm. Ultraviolet rays can be divided into three bands: near ultraviolet UVA: 315-400nm, far ultraviolet UVB: 280-315nm, and ultra-short ultraviolet UVC: 180-280nm. Ultraviolet rays account for about 6% of sunlight, of which the UVA band accounts for a larger proportion of the entire ultraviolet band, while the proportion of UVB is relatively small. It is well known that the ozone layer in the air has the function of protecting the earth's creatures, but with the deterioration of the ecological environment, the ozone layer in the atmosphere has been damaged, which has led to an increase in ultraviolet rays reaching the earth's surface. The increase in ultraviolet rays will pose a serious threat to human health and other creatures on the earth. Ultraviolet light and some visible light can also destroy the chemical bonds in organic macromolecules, thus leading to the degradation of organic matter and shortening the service life of the material. Since polyethylene terephthalate has excellent chemical and mechanical properties, it is widely used in aerospace and textile fields. Long-term use causes polyethylene terephthalate to be exposed to sunlight for a long time, which greatly shortens its service life. In order to avoid the harm of ultraviolet rays to the human body and the degradation of polymer materials, it is very necessary to carry out relevant anti-ultraviolet treatment.
[0003] The patent with application number CN201610720250.1 discloses a high-strength UV-resistant PE / PET composite material and its preparation method, which is composed of high-density polyethylene, ethylene terephthalate, interfacial compatibilizer, ultraviolet absorber and antioxidant; maleic anhydride and glycidyl methacrylate are selected as grafting monomers, which greatly improves the compatibility of polyolefin and ethylene terephthalate and avoids the reduction of grafting efficiency due to homopolymerization of monomers. The patent with application number CN202310114873.4 discloses a modified PET composite material and its preparation method, which is composed of PET, PC, trimethylolpropane triglycidyl ether, antioxidant, modified clay and lubricant; by using trimethylolpropane triglycidyl ether to blend with PET and PC, on the one hand, PET and PC can be cross-linked, the tensile strength and impact strength of the composite material can be improved, and the brittleness of the composite material can be reduced; on the other hand, the introduction of trimethylolpropane triglycidyl ether can improve the toughness of the PET composite material. However, in the above preparation process, the raw materials are directly mixed, which easily causes uneven mixing of the raw materials. Summary of the invention
[0004] In view of the deficiencies of the existing problems, the present invention provides an ultraviolet resistant polymer composite material and a preparation method thereof to solve the problems existing in the prior art.
[0005] The technical solution adopted by the present invention to solve the above technical problems is:
[0006] The invention discloses an ultraviolet-proof polymer composite material, which is composed of the following raw materials in parts by weight: 60-75 parts of modified polyethylene terephthalate, 12-20 parts of modified nanoparticles, 3-6 parts of antioxidants, 2-4 parts of heat stabilizers, and 1-2 parts of lubricants; preferably, the material comprises 72 parts of modified polyethylene terephthalate, 15 parts of modified nanoparticles, 4 parts of antioxidants, 3 parts of heat stabilizers, and 1 part of lubricants.
[0007] Furthermore, the antioxidant is one or more of antioxidant 1010, antioxidant TNP and antioxidant TPP, preferably antioxidant TNP; the heat stabilizer is zinc stearate; the lubricant is one or more of pentaerythritol stearate and ethylene bis stearamide, preferably pentaerythritol stearate.
[0008] Furthermore, the preparation method of the modified polyethylene terephthalate is as follows: after dissolving polyethylene terephthalate in dimethyl sulfoxide, 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol and an initiator are added thereto, heating and stirring the reaction at 75-85° C. for 20-24 hours, washing with deionized water and filtering after completion, washing with acetone for 2-3 times, and drying the product in a vacuum drying oven at 55-65° C. to constant weight to obtain the modified polyethylene terephthalate; wherein the initiator is one of potassium persulfate, benzoyl peroxide, and azobisisobutyronitrile, preferably benzoyl peroxide.
[0009] Under the action of heat, the covalent bond of the initiator breaks to generate free radicals to initiate a monomer with a double bond structure. Under the action of the initiator, the monomer 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol with ultraviolet absorption performance is grafted onto polyethylene terephthalate, achieving a bond-to-bond combination. Compared with the modification method of direct mixing, the bonding force combination is more solid; 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol as an ultraviolet absorber can effectively absorb ultraviolet rays with a wavelength of 310-385nm, has a wide absorption wavelength range and a high absorption index, and has a strong absorption capacity in the ultraviolet range. Before irradiation with external light, the hydroxyl group on the benzene ring mainly exists in the form of phenolic hydroxyl group. Since the electronegativity of the oxygen atom is greater than that of the nitrogen atom, the electron cloud density on the oxygen is higher than that of the nitrogen atom on the triazole, so that the hydroxyl group carries a certain amount of negative charge and exhibits alkaline characteristics. After absorbing ultraviolet light, most of the electrons are transferred from the oxygen atom to the nitrogen atom on the triazole, so that the hydroxyl group has a certain positive charge and shows a certain acidity. On the contrary, the nitrogen atom on the triazole shows a certain alkalinity, so that tautomers can be formed, which can convert the absorbed ultraviolet light into heat, release it in the form of energy, and return to the ground state, realizing repeated recycling.
[0010] Furthermore, the preparation method of the modified nanoparticles is as follows: the nanoparticles ZnO are dried and then ultrasonically dispersed in anhydrous ethanol for 20-40 minutes to obtain a nanoparticle dispersion liquid, a silane coupling agent is dispersed in an ethanol aqueous solution, the uniformly dispersed silane coupling agent solution is slowly added to the nanoparticle dispersion liquid under stirring and ultrasonically dispersed for 20-40 minutes, the obtained slurry is filtered, washed, and dried in a vacuum drying oven at 75-85° C. for 4-6 hours to obtain the modified nanoparticles; wherein the preparation method of the ethanol aqueous solution is as follows: distilled water and anhydrous ethanol are mixed at a volume ratio of 7-9:1; and the silane coupling agent is KH550.
[0011] Nano ZnO particles are modified by using a silane coupling agent. As a bifunctional substance, the hydrophilic part of the silane coupling agent can be combined with the inorganic nano ZnO particles, while the lipophilic part can penetrate into the polymer when mixed with the modified polyethylene terephthalate, and the nano ZnO particles can be well dispersed in the modified polyethylene terephthalate by entanglement with the polymer chain or the action of intermolecular force. Nano ZnO is used as an ultraviolet absorber, and its ultraviolet absorption comes from the energy level transition of electrons. Electrons in the ground state gather in the low-energy valence band. Once exposed to ultraviolet radiation, these electrons will absorb photon energy that can make them transition to the high-energy conduction band, and then release the absorbed energy in the form of heat or long-wavelength light radiation, thereby showing excellent ultraviolet shielding performance.
[0012] The present invention also provides a method for preparing an ultraviolet-proof polymer composite material, the preparation process of which is as follows:
[0013] S1. Mix the modified polyethylene terephthalate, modified nanoparticles, antioxidant, heat stabilizer and lubricant in a high-pressure mixer according to weight ratio;
[0014] S2. After the materials are evenly mixed, they are put into the feeding hopper of a twin-screw extruder, mixed and plasticized by the twin-screw extruder, extruded, cooled, and granulated;
[0015] S3, drying the pellets obtained in step S2 and then injection molding them into standard specimens to obtain an ultraviolet resistant polymer composite material.
[0016] Furthermore, the process parameters of the twin-screw extruder are: zone one temperature 190-200°C, zone two temperature 210-220°C, zone three temperature 230-250°C, zone four temperature 255-265°C, zone five temperature 265-275°C, zone six temperature 255-265°C, zone seven temperature 250-260°C, zone eight temperature 240-250°C, die head temperature 255-270°C, and screw speed 250-350rpm.
[0017] The present invention has the following beneficial effects:
[0018] The invention uses polyethylene terephthalate as a raw material, and generates a grafting reaction with 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol under the action of an initiator. The two are combined by bonding force, and compared with direct blending, the combination is more firm and the dispersion is more uniform. Meanwhile, modified nanoparticle ZnO is introduced in the preparation process, and the inorganic nanoparticle ZnO is modified by a silane coupling agent, and the hydrophilic part of the modified polyethylene terephthalate can be connected with the inorganic nanoparticle ZnO, and the lipophilic part can penetrate into the modified polyethylene terephthalate and entangle with the polymer chain when mixed, so that the nanoparticles have good dispersibility. By simultaneously introducing an organic ultraviolet absorber and an inorganic ultraviolet absorber into the polymer, compared with the introduction of a single ultraviolet absorber, the anti-ultraviolet performance of the prepared product is effectively improved, and in the preparation process, the introduction of rigid groups such as benzene rings and the inorganic nanoparticle ZnO also improves the mechanical properties of the product. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0020] The polyethylene terephthalate used in the present invention was purchased from Shanghai MacLean Biochemical Technology Co., Ltd. (P885051), the nanoparticle ZnO was purchased from Nanjing Apre Nanomaterials Co., Ltd. (particle size 50 nm), and 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol was purchased from Aladdin Chemical Reagent Network. All reagents used were commercially available.
[0021] Example 1
[0022] The invention discloses an anti-ultraviolet polymer composite material, which is composed of the following raw materials in parts by weight: 72 parts of modified polyethylene terephthalate, 15 parts of modified nanoparticles, 4 parts of antioxidant, 3 parts of heat stabilizer and 1 part of lubricant; wherein the antioxidant is antioxidant TNP, the heat stabilizer is zinc stearate and the lubricant is pentaerythritol stearate.
[0023] The preparation method of modified polyethylene terephthalate is as follows: after dissolving 75 parts by weight of polyethylene terephthalate in 135 parts by weight of dimethyl sulfoxide, 80 parts by weight of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol and initiator benzoyl peroxide are added thereto, heating and stirring the reaction at 80°C for 24 hours, washing with deionized water and filtering after completion, and then washing with acetone for 3 times, and drying the product in a vacuum drying oven at 60°C to constant weight to obtain modified polyethylene terephthalate, and the grafting rate of the modified polyethylene terephthalate is 62%.
[0024] The preparation method of modified nanoparticles is as follows: 18 parts by weight of nanoparticle ZnO are dried and then ultrasonically dispersed in 30 parts by weight of anhydrous ethanol for 40 minutes to obtain a nanoparticle dispersion liquid; 1 part by weight of a silane coupling agent is dispersed in 24 parts by weight of an ethanol aqueous solution; the uniformly dispersed silane coupling agent solution is slowly added to the nanoparticle dispersion liquid under stirring and ultrasonically dispersed for 40 minutes; the obtained slurry is filtered, washed, and dried in a vacuum drying oven at 80°C for 6 hours to obtain the modified nanoparticles; wherein the preparation method of the ethanol aqueous solution is as follows: distilled water and anhydrous ethanol are mixed in a volume ratio of 9:1; and the silane coupling agent is KH550.
[0025] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0026] S1. Mix 72 parts by weight of modified polyethylene terephthalate, 15 parts by weight of modified nanoparticles, 4 parts by weight of antioxidant, 3 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0027] S2. After the materials are evenly mixed, they are put into the feeding hopper of a twin-screw extruder, mixed and plasticized by the twin-screw extruder, extruded, cooled, and granulated;
[0028] S3, drying the pellets obtained in step S2 and then injection molding them into standard specimens to obtain an ultraviolet resistant polymer composite material.
[0029] Among them, the process parameters of the twin-screw extruder are: zone 1 temperature 195°C, zone 2 temperature 215°C, zone 3 temperature 240°C, zone 4 temperature 260°C, zone 5 temperature 270°C, zone 6 temperature 260°C, zone 7 temperature 255°C, zone 8 temperature 245°C, die head temperature 265°C, and screw speed 300rpm.
[0030] Example 2
[0031] A UV-proof polymer composite material is composed of the following raw materials in parts by weight: 60 parts of modified polyethylene terephthalate, 12 parts of modified nanoparticles, 3 parts of antioxidants, 2 parts of heat stabilizers, and 1 part of lubricants; wherein the antioxidant is antioxidant 1010, the heat stabilizer is zinc stearate, and the lubricant is ethylene bis stearamide.
[0032] The preparation method of modified polyethylene terephthalate is as follows: after dissolving 62 parts by weight of polyethylene terephthalate in 120 parts by weight of dimethyl sulfoxide, 65 parts by weight of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol and initiator benzoyl peroxide are added thereto, heating and stirring the reaction at 75° C. for 22 hours, washing with deionized water and filtering after completion, and then washing with acetone twice, and drying the product in a vacuum drying oven at 55° C. to constant weight to obtain modified polyethylene terephthalate, and the grafting rate of the modified polyethylene terephthalate is 58%.
[0033] The preparation method of modified nanoparticles is as follows: 15 parts by weight of nanoparticle ZnO are dried and then ultrasonically dispersed in 25 parts by weight of anhydrous ethanol for 20 minutes to obtain a nanoparticle dispersion liquid, 0.8 parts by weight of a silane coupling agent is dispersed in 20 parts by weight of an ethanol aqueous solution, the uniformly dispersed silane coupling agent solution is slowly added to the nanoparticle dispersion liquid under stirring and ultrasonically dispersed for 20 minutes, the obtained slurry is filtered, washed, and dried in a vacuum drying oven at 75°C for 4 hours to obtain modified nanoparticles; wherein the preparation method of the ethanol aqueous solution is as follows: distilled water and anhydrous ethanol are mixed in a volume ratio of 7:1; and the silane coupling agent is KH550.
[0034] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0035] S1. Mix 60 parts by weight of modified polyethylene terephthalate, 12 parts by weight of modified nanoparticles, 3 parts by weight of antioxidant, 2 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0036] S2. After the materials are evenly mixed, they are put into the feeding hopper of a twin-screw extruder, mixed and plasticized by the twin-screw extruder, extruded, cooled, and granulated;
[0037] S3, drying the pellets obtained in step S2 and then injection molding them into standard specimens to obtain an ultraviolet resistant polymer composite material.
[0038] Among them, the process parameters of the twin-screw extruder are: zone 1 temperature 190°C, zone 2 temperature 210°C, zone 3 temperature 230°C, zone 4 temperature 255°C, zone 5 temperature 265°C, zone 6 temperature 255°C, zone 7 temperature 250°C, zone 8 temperature 240°C, die head temperature 255°C, and screw speed 250rpm.
[0039] Example 3
[0040] The invention discloses an anti-ultraviolet polymer composite material, which is composed of the following raw materials in parts by weight: 75 parts of modified polyethylene terephthalate, 20 parts of modified nanoparticles, 6 parts of antioxidant, 4 parts of heat stabilizer and 2 parts of lubricant; wherein the antioxidant is antioxidant TPP, the heat stabilizer is zinc stearate and the lubricant is pentaerythritol stearate.
[0041] The preparation method of modified polyethylene terephthalate is as follows: after dissolving 80 parts by weight of polyethylene terephthalate in 160 parts by weight of dimethyl sulfoxide, 85 parts by weight of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol and initiator benzoyl peroxide are added thereto, heating and stirring the reaction at 85° C. for 24 hours, washing with deionized water and filtering after completion, and then washing with acetone for 3 times, and drying the product in a vacuum drying oven at 65° C. to constant weight to obtain modified polyethylene terephthalate, and the grafting rate of the modified polyethylene terephthalate is 54%.
[0042] The preparation method of modified nanoparticles is as follows: 22 parts by weight of nanoparticle ZnO are dried and then ultrasonically dispersed in 45 parts by weight of anhydrous ethanol for 40 minutes to obtain a nanoparticle dispersion liquid; 1.5 parts by weight of a silane coupling agent are dispersed in 35 parts by weight of an ethanol aqueous solution; the uniformly dispersed silane coupling agent solution is slowly added to the nanoparticle dispersion liquid under stirring and ultrasonically dispersed for 40 minutes; the obtained slurry is filtered, washed, and dried in a vacuum drying oven at 85°C for 6 hours to obtain the modified nanoparticles; wherein the preparation method of the ethanol aqueous solution is as follows: distilled water and anhydrous ethanol are mixed in a volume ratio of 8:1; and the silane coupling agent is KH550.
[0043] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0044] S1. Mix 75 parts by weight of modified polyethylene terephthalate, 20 parts by weight of modified nanoparticles, 6 parts by weight of antioxidant, 4 parts by weight of heat stabilizer and 2 parts by weight of lubricant in a high-speed mixer;
[0045] S2. After the materials are evenly mixed, they are put into the feeding hopper of a twin-screw extruder, mixed and plasticized by the twin-screw extruder, extruded, cooled, and granulated;
[0046] S3, drying the pellets obtained in step S2 and then injection molding them into standard specimens to obtain an ultraviolet resistant polymer composite material.
[0047] Among them, the process parameters of the twin-screw extruder are: zone 1 temperature 200°C, zone 2 temperature 220°C, zone 3 temperature 250°C, zone 4 temperature 265°C, zone 5 temperature 275°C, zone 6 temperature 265°C, zone 7 temperature 260°C, zone 8 temperature 250°C, die head temperature 270°C, and screw speed 350rpm.
[0048] Comparative Example 1
[0049] Compared with Example 1, polyethylene terephthalate is not grafted and modified, and 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol is directly introduced. The rest of the process is the same as Example 1.
[0050] Specifically: an anti-ultraviolet polymer composite material, composed of the following raw materials in parts by weight: 72 parts of polyethylene terephthalate, 42 parts of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol, 15 parts of modified nanoparticles, 4 parts of antioxidant, 3 parts of heat stabilizer, and 1 part of lubricant; wherein the antioxidant is antioxidant TNP, the heat stabilizer is zinc stearate, and the lubricant is pentaerythritol stearate.
[0051] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0052] S1. Mix 72 parts by weight of polyethylene terephthalate, 42 parts by weight of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol, 15 parts by weight of modified nanoparticles, 4 parts by weight of antioxidant, 3 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0053] Steps S2 and S3 are the same as those in Example 1.
[0054] Comparative Example 2
[0055] Compared with Example 1, the nanoparticles are not modified, and the remaining processes refer to Example 1.
[0056] Specifically: an anti-ultraviolet polymer composite material, composed of the following raw materials in parts by weight: 72 parts of modified polyethylene terephthalate, 15 parts of nanoparticles, 4 parts of antioxidants, 3 parts of heat stabilizers, and 1 part of lubricants; wherein the antioxidant is antioxidant TNP, the heat stabilizer is zinc stearate, and the lubricant is pentaerythritol stearate.
[0057] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0058] S1. Mix 72 parts by weight of modified polyethylene terephthalate, 15 parts by weight of nanoparticles, 4 parts by weight of antioxidant, 3 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0059] Steps S2 and S3 are the same as those in Example 1.
[0060] Comparative Example 3
[0061] Compared with Example 1, polyethylene terephthalate is not grafted and modified, 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol is directly introduced, and the nanoparticles are not modified. The rest of the process is the same as Example 1.
[0062] Specifically: an anti-ultraviolet polymer composite material, composed of the following raw materials in parts by weight: 72 parts of polyethylene terephthalate, 42 parts of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol, 15 parts of nanoparticles, 4 parts of antioxidant, 3 parts of heat stabilizer, and 1 part of lubricant; wherein the antioxidant is antioxidant TNP, the heat stabilizer is zinc stearate, and the lubricant is pentaerythritol stearate.
[0063] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0064] S1. Mix 72 parts by weight of polyethylene terephthalate, 42 parts by weight of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol, 15 parts by weight of nanoparticles, 4 parts by weight of antioxidant, 3 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0065] Steps S2 and S3 are the same as those in Example 1.
[0066] Comparative Example 4
[0067] Compared with Example 1, polyethylene terephthalate is not modified during the preparation process, and the remaining processes refer to Example 1.
[0068] Specifically:
[0069] The invention discloses an ultraviolet-proof polymer composite material, which is composed of the following raw materials in parts by weight: 72 parts of polyethylene terephthalate, 15 parts of modified nanoparticles, 4 parts of antioxidants, 3 parts of heat stabilizers and 1 part of lubricants.
[0070] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0071] S1. Mix 72 parts by weight of polyethylene terephthalate, 15 parts by weight of modified nanoparticles, 4 parts by weight of antioxidant, 3 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0072] Steps S2 and S3 are the same as those in Example 1.
[0073] Comparative Example 5
[0074] Compared with Example 1, no modified nanoparticles were added during the preparation process, and the remaining processes were referred to Example 1.
[0075] A UV-proof polymer composite material is composed of the following raw materials in parts by weight: 72 parts of modified polyethylene terephthalate, 4 parts of antioxidant, 3 parts of heat stabilizer and 1 part of lubricant; wherein the antioxidant is antioxidant TNP, the heat stabilizer is zinc stearate and the lubricant is pentaerythritol stearate.
[0076] A method for preparing an ultraviolet-proof polymer composite material, the preparation process comprising:
[0077] S1. Mix 72 parts by weight of modified polyethylene terephthalate, 4 parts by weight of antioxidant, 3 parts by weight of heat stabilizer and 1 part by weight of lubricant in a high-speed mixer;
[0078] Steps S2 and S3 are the same as those in Example 1.
[0079] Performance Testing
[0080] The performance tests were carried out on the samples prepared in Examples 1-3 and Comparative Examples 1-5: Tensile strength: measured according to ASTM D638, and the test conditions were 50 mm / min; Izod notched impact strength: measured according to ASTM D256, and the test conditions were: using a 3.2 mm thick film notched Izod impact bar, 23°C; Flexural strength: measured according to ASTM D790, and the test conditions were 2 mm / min; the test results are shown in Table 1.
[0081] Table 1
[0082]
[0083] The samples prepared in Examples 1-3 and Comparative Examples 1-5 were subjected to an ultraviolet aging experiment: the samples were placed in an ultraviolet lamp box with a wavelength range of 250-380 nm and a power of 1000 W for irradiation. The sample was 15 cm away from the lamp tube and the temperature in the lamp box was 70°C. In order to ensure uniform irradiation on both sides of the sample, all the sample strips were turned over once every 10 minutes. The irradiation time of the sample strips was 2 h. The difference between the mechanical property data before aging and the mechanical property data after aging was calculated, which was the mechanical property reduction value. The results are shown in Table 2.
[0084] Table 2
[0085]
[0086]
[0087] The light blocking performance of the samples prepared in Examples 1-3 and Comparative Examples 1-5 was tested using an ultraviolet visible spectrophotometer UV-2700 produced by Shimadzu Corporation of Japan; before the test, the products prepared in each Example and Comparative Example were prepared into a film with a thickness of about 15 μm and cut into a size of 5 cm×5 cm, and the cut samples were fixed on the sample holder before the test; then the instrument was turned on and preheated for a few minutes, and then the corresponding software was opened to set the relevant parameters, with air permeability as a reference, the scanning range was set to 200-400 nm, the scanning speed was medium speed, the scanning mode was single, the sampling interval was set between 0.5-2.0, and the measurement method was transmittance. The test results are shown in Table 3 (wherein the control sample is pure polyethylene terephthalate).
[0088] Table 3
[0089]
[0090] The test results in Tables 1-3 show that the relevant performances of the embodiments are better than those of the comparative examples, among which the test results of Embodiment 1 are the best; by comparing the test results of Embodiment 1 with those of Comparative Example 1 (polyethylene terephthalate is not grafted and modified), Comparative Example 2 (nanoparticles are not modified) and Comparative Example 3 (direct introduction of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol and nanoparticles), it can be found that: compared with directly adding 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol to the raw materials, grafting it onto the polyethylene terephthalate molecular chain through reaction can further improve the mechanical properties and anti-ultraviolet properties of the prepared composite material; in addition, the lipophilic part of the modified nanoparticle ZnO can penetrate into the interior of the polymer, promote the dispersion of the nanoparticle ZnO, and effectively prevent it from agglomerating during the mixing process. By comparing the test results of Example 1 with Comparative Example 4 (without the introduction of 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol) and Comparative Example 5 (without the introduction of modified nanoparticles), it can be found that the simultaneous introduction of an organic ultraviolet absorber (2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol) and an inorganic ultraviolet absorber (modified nanoparticle ZnO) can achieve a better ultraviolet absorption effect.
[0091] The invention uses polyethylene terephthalate as a raw material, and a grafting reaction is carried out with 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol under the action of an initiator. The two are combined by bonding force, and the combination is more firm and the dispersion is more uniform compared with direct blending. Before absorbing light, the grafted 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol exists in the form of phenol compounds. Since the electron cloud density on the oxygen atom is much greater than the electron cloud density on the nitrogen atom of the triazole ring, it presents strong alkalinity. After absorbing light, the electron density is transferred from the oxygen atom to the nitrogen atom, so that the phenol has acidity and the nitrogen atom has more alkalinity. The proton is quickly transferred to the nitrogen atom to form a tautomer. Since the tautomer is unstable, the excess energy is converted into heat energy to return to a more stable ground state. Since the interconversion process is extremely efficient, it can be infinitely repeated, so that it has good light stability. At the same time, Modified nanoparticles ZnO are also introduced in the preparation process. The inorganic nanoparticles ZnO are modified by using a silane coupling agent. The hydrophilic part of the hydrophilic part can be connected to the inorganic nanoparticles ZnO, and the lipophilic part can penetrate into the modified polyethylene terephthalate and entangle with the polymer chain when mixed with the modified polyethylene terephthalate, so that the nanoparticles have good dispersibility. The inorganic nanoparticles ZnO are excellent inorganic ultraviolet absorbers. After being irradiated with ultraviolet radiation, the electrons in the ground state gathered in the low-energy valence band absorb photon energy and transition to the high-energy conduction band, and then release the absorbed energy in the form of heat or long-wavelength radiation, thereby showing excellent ultraviolet shielding performance. By simultaneously introducing organic ultraviolet absorbers and inorganic ultraviolet absorbers into the polymer, compared with the introduction of a single ultraviolet absorber, the anti-ultraviolet performance of the prepared product is effectively improved, and in the preparation process, the introduction of rigid groups such as benzene rings and inorganic nanoparticles ZnO also improves the mechanical properties of the product.
[0092] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0093] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A UV-proof polymer composite material, characterized in that: The invention is composed of the following raw materials in parts by weight: 60-75 parts of modified polyethylene terephthalate, 12-20 parts of modified nanometer particles, 3-6 parts of antioxidant, 2-4 parts of heat stabilizer and 1-2 parts of lubricant.
2. The ultraviolet resistant polymer composite material according to claim 1, characterized in that: The preparation method of the modified polyethylene terephthalate comprises the following steps: dissolving polyethylene terephthalate in dimethyl sulfoxide, adding 2-allyl-6-(2H-benzotriazole-2-yl)-4-methylphenol and an initiator, heating and stirring the mixture to react, washing with deionized water, filtering the mixture, and then washing with acetone, and drying the product to a constant weight to obtain the modified polyethylene terephthalate.
3. The ultraviolet protection polymer composite material according to claim 1, characterized in that: The preparation method of the modified nanoparticles comprises: drying the nanoparticles and then ultrasonically dispersing them in anhydrous ethanol to obtain a nanoparticle dispersion liquid; dispersing a silane coupling agent in an ethanol aqueous solution, adding the silane coupling agent to the nanoparticle dispersion liquid under stirring and ultrasonically dispersing the silane coupling agent; and filtering, washing and drying the obtained slurry to obtain the modified nanoparticles.
4. The ultraviolet protection polymer composite material according to claim 2, characterized in that: The initiator is one of potassium persulfate, benzoyl peroxide and azobisisobutyronitrile.
5. The ultraviolet resistant polymer composite material according to claim 2, characterized in that: The conditions for heating and stirring are: reacting at 75-85°C for 20-24h, and the conditions for drying the product are: drying in a vacuum drying oven at 55-65°C to constant weight.
6. The ultraviolet protection polymer composite material according to claim 3, characterized in that: The nanoparticles are ZnO nanoparticles.
7. The ultraviolet protection polymer composite material according to claim 3, characterized in that: The nanoparticles were dried in a vacuum oven at 75-85°C for 4-6 hours.
8. The ultraviolet protection polymer composite material according to claim 3, characterized in that: The preparation method of the ethanol aqueous solution is: mixing distilled water and anhydrous ethanol in a volume ratio of 7-9:
1.
9. The method for preparing an ultraviolet resistant polymer composite material according to any one of claims 1 to 8, characterized in that: The preparation process is: S1. Mix the modified polyethylene terephthalate, modified nanoparticles, antioxidant, heat stabilizer and lubricant in a high-pressure mixer according to weight ratio; S2. After the materials are evenly mixed, they are put into the feeding hopper of a twin-screw extruder, mixed and plasticized by the twin-screw extruder, extruded, cooled, and granulated; S3, drying the pellets obtained in step S2 and then injection molding them into standard specimens to obtain an ultraviolet resistant polymer composite material.
Citation Information
Cited By
Composite material for improving UV resistance of HDPE (high-density polyethylene) and preparation method of composite material
CN119552446A