Degradable cooling filter stick material, preparation method thereof and cigarette

Through the combination of modified polylactic acid, cellulose and stabilizer, the problem of excessive temperature and environmental pollution of cigarette filter rod materials during smoking is solved, and better thermal stability and degradability are achieved.

CN118791853APending Publication Date: 2024-10-18HUBEI CHINA TOBACCO INDUSTRY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410859237.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The temperature of existing cigarette filter rod materials is too high during smoking, resulting in weak support and difficulty in rapid degradation in the natural environment, causing environmental pollution.

Method used

Using a combination of modified polylactic acid, modified cellulose and stabilizer, by adding new nucleating agents and radiation-modified cellulose, the crystallinity and compatibility of the material are improved, and its heat resistance and mechanical properties are enhanced. And the cooling filter rod material is made by extrusion preparation method.

Benefits of technology

It improves the thermal stability and supporting force of the filter rod material, reduces the temperature during smoking, and can be quickly degraded in the natural environment, reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004918843110000021
    Figure BDA0004918843110000021
  • Figure BDA0004918843110000041
    Figure BDA0004918843110000041
  • Figure BDA0004918843110000101
    Figure BDA0004918843110000101
Patent Text Reader

Abstract

The invention provides a degradable cooling filter stick material. The degradable cooling filter stick material is prepared from the following raw materials in parts by weight: 30-60 parts of modified polylactic acid, 30-60 parts of modified cellulose and 1-2 parts of a stabilizer. Compared with an existing filter rod material, the glass-transition temperature of the filter rod material provided by the invention is increased, so that the thermal stability of the COO smoke cartridge after being heated is improved, the deformation of the COO smoke cartridge in the use process is reduced, and the problem that the supporting property of the smoke cartridge after being smoked and heated is not strong is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cigarette filter rod materials, in particular to a degradable cooling filter rod material and a preparation method thereof and a cigarette. Background Art

[0002] At present, the materials used to make cigarette filter rods are generally cellulose acetate fiber and polypropylene fiber. Considering the processing performance and the comprehensive performance of the final filter tip, cellulose acetate fiber is the first choice. Cellulose acetate fiber is difficult to be biodegraded in the natural environment, causing environmental pollution. Therefore, solving the environmental pollution problem caused by discarded filter tips has become an important issue that the cigarette industry must face.

[0003] Lactic acid polymers are biodegradable and can meet the requirements of filter rod processing, and are applied in the field of cigarette filter rod material technology. Patent CN102080278B discloses a biodegradable cigarette fiber material and a cigarette filter. The raw materials are composed of polybutylene succinate polymer, 1-polylactic acid polymer and stabilizer. The prepared filter can be decomposed in a short time in the natural environment. While meeting the requirements of cigarette production, it also solves the pollution effect of current cigarette waste on the environment. However, it does not take into account the high temperature of smoke entering the oral cavity and the taste problem during inhalation. Patent CN110643158B discloses a polylactic acid foaming material for cigarette filter. The raw materials are mainly composed of polylactic acid resin, polyester elastomer, citric acid, sodium bicarbonate, surfactant, composite stabilizer, release agent, foaming agent and foaming aid by weight. The prepared polylactic acid foaming material has a high foaming ratio, a large porosity, and is not prone to belt breakage during the molding process. However, the degradation rate of polyester is slow, which will cause environmental pollution.

[0004] Therefore, there is an urgent need for a degradable cooling filter rod material that can cool down and satisfy people's smoking taste. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a degradable cooling filter rod material. The filter rod material provided by the present invention can solve the problem of weak supporting force after suction and heating, and at the same time has a cooling effect.

[0006] The present invention provides a degradable cooling filter rod material, comprising the following raw materials in parts by weight:

[0007] 30-60 parts of modified polylactic acid, 30-60 parts of modified cellulose and 1-2 parts of stabilizer.

[0008] Preferably, the preparation method of the modified polylactic acid comprises:

[0009] The nucleating agent and polylactic acid are mixed and kneaded, and extruded and granulated to obtain modified polylactic acid;

[0010] The mass ratio of the polylactic acid to the nucleating agent is 1:(0.005-0.01);

[0011] The temperature of the banburying is 170-190° C., the speed of the banburying is 55-65 r / min, and the time of the banburying is 5-10 min.

[0012] Preferably, the nucleating agent is represented by the structure of formula (I):

[0013]

[0014] Preferably, the preparation method of the nucleating agent comprises:

[0015] Add 1,6-hexanediamine and p-toluenesulfonyl isocyanate to N,N-dimethylformamide, stir to react, and separate to obtain;

[0016] The reaction temperature is 30-40°C, and the stirring time is 55-65min;

[0017] The mass ratio of the 1,6-hexanediamine to p-toluenesulfonyl isocyanate is 1:(3.4-3.7).

[0018] Preferably, the preparation of the modified cellulose comprises:

[0019] The cellulose is dissolved in a solvent, mixed with a polyvinyl alcohol aqueous solution, stirred, vacuum irradiated, and dried to obtain the cellulose; the solvent includes N,N-dimethylacetamide;

[0020] The stirring time is 8 to 10 minutes.

[0021] Preferably, the mass ratio of the polyvinyl alcohol to the cellulose is (0.05-0.15):1;

[0022] The vacuum degree of the vacuum irradiation is 0.08-0.1MPa; the irradiation source is an electron accelerator, and the irradiation dose is 1-5KGy.

[0023] Preferably, the stabilizer is selected from any one of epoxidized linseed oil and epoxidized soybean oil.

[0024] The present invention provides a method for preparing a cooling filter rod material, comprising the following steps:

[0025] The modified polylactic acid, modified cellulose and stabilizer are uniformly mixed, extruded, pelletized and dried to obtain the product.

[0026] The present invention provides a cigarette filter rod, the raw material of which includes the degradable cooling filter rod material described in any one of the above technical solutions.

[0027] The present invention provides a cigarette, comprising the cigarette filter rod described in the above technical solution.

[0028] Compared with the prior art, the present invention provides a degradable cooling filter rod material, comprising the following raw materials in parts by weight: 30-60 parts of modified polylactic acid, 30-60 parts of modified cellulose and 1-2 parts of stabilizer. Compared with the existing filter rod material, the filter rod material provided by the present invention has a higher glass transition temperature, thereby improving the thermal stability of the COO cigarette cartridge after being heated, reducing its deformation during use, and solving the problem of weak support after the cigarette cartridge is heated during smoking. DETAILED DESCRIPTION

[0029] The present invention provides a degradable cooling filter rod material and a preparation method thereof and a cigarette. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the desired effect. It should be particularly noted that all similar replacements and modifications are obvious to those skilled in the art and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to achieve and apply the technology of the present invention.

[0030] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0031] In this application, "at least one" means one or more, "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items.

[0032] The present invention provides a degradable cooling filter rod material, comprising the following raw materials in parts by weight:

[0033] 30-60 parts of modified polylactic acid, 30-60 parts of modified cellulose and 1-2 parts of stabilizer.

[0034] In one embodiment of the present invention, the degradable cooling filter rod material comprises the following raw materials in parts by weight:

[0035] 45 parts of modified polylactic acid, 45 parts of modified cellulose and 1.5 parts of stabilizer.

[0036] In one embodiment of the present invention, the degradable cooling filter rod material comprises the following raw materials in parts by weight:

[0037] 30 parts of modified polylactic acid, 30 parts of modified cellulose and 1 part of stabilizer.

[0038] In one embodiment of the present invention, the degradable cooling filter rod material comprises the following raw materials in parts by weight:

[0039] 60 parts of modified polylactic acid, 60 parts of modified cellulose and 2 parts of stabilizer.

[0040] According to the present invention, the preparation method of the modified polylactic acid comprises:

[0041] The nucleating agent and polylactic acid are mixed and kneaded, and then extruded and granulated to obtain modified polylactic acid.

[0042] The temperature of the banburying of the present invention is 170-190°C, more preferably 175-185°C, and most preferably 180°C; the speed of the banburying is 55-65r / min, more preferably 57-63r / min, and most preferably 60r / min. The time of banburying (melt blending) is 5-10min, preferably 6-9min, and more preferably 8-9min.

[0043] The nucleating agent of the present invention is shown in the structure of formula (I):

[0044]

[0045] In some embodiments, the mass ratio of polylactic acid to nucleating agent is 1:(0.005-0.01), which may be specifically 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009 or 1:0.01, or any value between the above two.

[0046] In one of the embodiments, the mass ratio of polylactic acid to nucleating agent is 1:0.008.

[0047] According to the present invention, the preparation method of the nucleating agent comprises:

[0048] Add 1,6-hexanediamine and p-toluenesulfonyl isocyanate into N,N-dimethylformamide, stir to react, and separate to obtain the product.

[0049] In the present invention, the mass ratio of the 1,6-hexanediamine to p-toluenesulfonyl isocyanate is 1:(3.4-3.7).

[0050] The mass ratio of 1,6-hexanediamine to p-toluenesulfonyl isocyanate of the present invention is 1:3.4, 1:3.5, 1:3.6 or 1:3.7; or a value between any two of the above.

[0051] In some embodiments, the mass ratio of hexamethylenediamine to p-toluenesulfonyl isocyanate is 1:3.6.

[0052] The reaction temperature of the present invention is 30-40°C, and the stirring time is 55-65min; preferably, the reaction temperature is 32-38°C, and the stirring time is 57-63min; more preferably, the reaction temperature is 35-36°C, and the stirring time is 59-60min.

[0053] The present invention does not limit the separation after stirring, and it can be well known to those skilled in the art.

[0054] Polylactic acid is a polymer material with excellent properties that can be extracted from bio-renewable resources, does not cause pollution to the environment, can be completely degraded by microorganisms in the natural environment, is non-irritating to the human body, and is not prone to allergies. It has potential application value in various fields. However, due to its slow crystallization rate and low crystallinity, polylactic acid has disadvantages such as long molding cycle, insufficient mechanical properties, and poor heat resistance, which greatly inhibits the application and development of polylactic acid. Therefore, improving the crystallization properties of polylactic acid is an important issue that needs to be urgently solved to expand the practical application areas of polylactic acid.

[0055] The applicant has found that the crystallinity of PLA can be improved by adding a nucleating agent, thereby improving its mechanical properties and heat resistance. The nucleating agent can be divided into an inorganic nucleating agent and an organic nucleating agent. The commonly used inorganic nucleating agents such as talcum powder, montmorillonite, calcium carbonate, etc. have poor compatibility with PLA and uneven dispersion, resulting in poor mechanical properties of polylactic acid, which limits its application. The organic nucleating agent has good compatibility with PLA and can be added in a smaller amount to obtain a better nucleating effect. The present invention uses 1,6-hexanediamine and p-toluenesulfonyl isocyanate to prepare a new polylactic acid nucleating agent. The nucleating agent molecule has 4 NH bonds. The electron-withdrawing ability of N is greater than that of H, resulting in the shared electron pair being biased toward the N atom away from the H atom, so that the H on the NH bond and the PLA The C=O on the nucleating agent interacts to form hydrogen bonds. The nucleating agent and PLA are connected by hydrogen bonds, which provide nucleation sites for PLA crystallization during the crystallization process. The adsorbed molecular chains are arranged in order to form attached crystals. In addition, there are other groups between the four NH groups, which reduces the agglomeration of polylactic acid and improves the crystallinity of PLA, thereby improving its heat resistance and glass transition temperature. At the same time, the mass ratio between the nucleating agent and polylactic acid is controlled to prevent the aggregation of the nucleating agent from affecting the crystallization of polylactic acid, further improving the problem of polylactic acid softening when heated and also improving the mechanical properties. In addition, the sulfonyl group on the nucleating agent has a strong polarity and can react chemically with tar components and low molecular weight substances to fix them in the filter tip, reducing harm to the human body.

[0056] According to the present invention, the preparation of the modified cellulose comprises:

[0057] The cellulose is dissolved in a solvent, mixed with a polyvinyl alcohol aqueous solution, stirred, vacuum irradiated, and dried to obtain the product.

[0058] The solvent includes N,N-dimethylacetamide, the cellulose is nanocellulose, and the particle size is 3-10 nm. The stirring time is 8-10 min, specifically 8 min, 9 min or 10 min, or any value between the above two.

[0059] According to the present invention, the mass ratio of polyvinyl alcohol to cellulose is (0.05-0.15):1; specifically, it can be 0:05:1, 0:06:1, 0:07:1, 0:08:1, 0:09:1, 0:10:1, 0:11:1, 0:12:1, 0:13:1, 0:14:1, 0:15:1, or any point value between any two of the above.

[0060] In some embodiments, the mass ratio of polyvinyl alcohol to cellulose is 0.08:1.

[0061] The vacuum degree of the vacuum irradiation of the present invention is 0.08 to -0.1 MPa; the irradiation source is an electron accelerator, and the irradiation dose is 1 to 5 KGy; specifically, it can be 1 KGy, 2 KGy, 3 KGy, 4 KGy or 5 KGy; or a point value between any two of the above.

[0062] The concentration of the polyvinyl alcohol aqueous solution is 8 wt %; the mass ratio of the cellulose to the solvent is 1:10.

[0063] Cellulose is a natural biomass material that is naturally degradable and does not pollute the environment. It can also be regenerated through plant growth and is a renewable material that will not dry up. Cellulose material has excellent wear resistance, is durable, and is not easily damaged. The processed cellulose material has high strength and can be used in a variety of fields such as manufacturing high-strength textiles and building materials.

[0064] The applicant found that the rich functional groups on the surface of cellulose provide a variety of possibilities for chemical modification, and thus provide more sites for cross-linking between structural units, which is conducive to enhancing interactions and improving mechanical strength. In addition, the glucose molecules inside the cellulose are arranged closely in a linear manner, giving it excellent toughness. Therefore, cellulose can be used to improve the brittleness of polylactic acid after processing. However, the compatibility between polylactic acid and cellulose is poor. Direct modification with cellulose may result in loose bonding and uneven molecules inside the material, affecting the quality of the material. The present invention uses polyvinyl alcohol to irradiate and modify cellulose. Polyvinyl alcohol has good compatibility with polylactic acid, thereby improving the problem of poor compatibility between polylactic acid and cellulose. Compared with traditional methods (such as heat treatment, chemical modification, etc.), the irradiation modification technology can complete the modification of materials in a shorter time, greatly improving the production efficiency. No harmful substances will be generated during the modification process. By adjusting the radiation parameters, accurate control of material modification can be achieved to meet the special needs of different products. After irradiation, the glycosidic bonds in the cellulose are broken to generate free radicals, which react with the hydroxyl groups of the polyvinyl alcohol. The two are connected through a -COO- bond, thereby improving the compatibility of polylactic acid and cellulose. In addition, the polyvinyl alcohol has good water absorption, and can fix the water vapor generated by heating tobacco to prevent the smoke inhaled into the mouth from being too hot. In addition, compared with irradiating with radioactive isotopes, irradiating samples with high-energy electrons will not cause radioactive pollution to the environment. The high-energy electrons have an irradiation effect only when the power supply is connected, and there is no radioactive residue. At the same time, the sample will be heated during irradiation. While the sample undergoes a chemical reaction, its own temperature gradually rises, thereby improving the reaction efficiency.

[0065] The stabilizer of the present invention is selected from any one of epoxidized linseed oil and epoxidized soybean oil.

[0066] The present invention provides a method for preparing a cooling filter rod material, comprising the following steps:

[0067] The modified polylactic acid, modified cellulose and stabilizer are uniformly mixed, extruded, pelletized and dried to obtain the product.

[0068] The extrusion temperature of the present invention is 180-220° C., specifically 180° C., 190° C., 200° C., 210° C., 220° C., or any point value between the above two.

[0069] The present invention does not limit the pelletizing and drying, which are well known to those skilled in the art.

[0070] The present invention provides a cigarette filter rod, the raw material of which includes the degradable cooling filter rod material described in any one of the above technical solutions.

[0071] The present invention has already clearly described the above-mentioned degradable cooling filter rod material, which will not be repeated here.

[0072] The present invention provides a cigarette, comprising the cigarette filter rod described in the above technical solution.

[0073] Cigarettes of the present invention refer to any product that can be smoked, whether based on tobacco, tobacco derivatives, expanded tobacco, reconstituted tobacco or tobacco substitutes, or any product that can provide a smoking experience. For example, smoking articles may include smokable articles, such as ordinary cigarettes, cigars and cigarillos. As another example, smoking articles may include combustion smoking articles and heated smoking articles.

[0074] Compared with the prior art, the present invention has the following beneficial effects:

[0075] 1. The filter rod material obtained by the present invention through preparing a new nucleating agent and modified cellulose can solve the problem that the conventional polylactic acid filter rod material has weak supporting force after being heated during suction, and at the same time has a cooling effect.

[0076] 2. The present invention utilizes 1,6-hexanediamine and p-toluenesulfonyl isocyanate to prepare a novel polylactic acid nucleating agent, which improves the crystallinity of PLA, thereby improving its heat resistance and glass transition temperature, and at the same time controls the mass ratio between the nucleating agent and the polylactic acid, further improves the problem of the polylactic acid becoming soft when heated, and also improves the mechanical properties; in addition, the sulfonyl group on the nucleating agent has a strong polarity, and can react chemically with tar components and low molecular weight substances to fix them in the filter, thereby reducing harm to the human body.

[0077] 3. The present invention uses polyvinyl alcohol to irradiate and modify cellulose. Polyvinyl alcohol has good compatibility with polylactic acid, thus improving the problem of poor compatibility between polylactic acid and cellulose. At the same time, polyvinyl alcohol has good water absorption and can fix the water vapor generated by heating tobacco to prevent the smoke inhaled into the mouth from being too hot.

[0078] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0079] The numerical ranges and parameters involved in the present invention have presented the relevant numerical values ​​in the specific embodiments as accurately as possible. However, any numerical value essentially inevitably contains standard deviations due to individual testing methods. Therefore, unless otherwise explicitly stated, it should be understood that all numerical ranges or specific data used in this disclosure may have certain reasonable deviations within a certain range, for example: within 1% or 0.5%.

[0080] Some cases are recorded in the embodiments and comparative examples of the present invention, wherein the embodiments show certain implementation modes of the present invention. However, this does not mean that the effects of the present invention can only be achieved in these cases.

[0081] In order to further illustrate the present invention, a degradable cooling filter rod material, a preparation method thereof and a cigarette provided by the present invention are described in detail below in conjunction with examples.

[0082] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows:

[0083] Polylactic acid was purchased from Shanghai Yien Chemical Technology Co., Ltd. with a number average molecular weight of 60,000;

[0084] Polyvinyl alcohol was purchased from Tianjin Xiensi Biochemical Technology Co., Ltd., with alcoholysis degree: 85.0-90.0 mol%, viscosity: 20.0-30.0 mPa·S;

[0085] Nanocellulose was purchased from Hubei Shineng Chemical Technology Co., Ltd. with a particle size of 3-10 nm;

[0086] Cellulose was purchased from Shenyang Elex Chemical Co., Ltd. with a purity of 99%;

[0087] The nucleating agent sebacic acid diphenyl dihydrazide SDA356 was purchased from Dongguan Shengde New Materials Co., Ltd.

[0088] Preparation Example 1

[0089] The preparation method of the nucleating agent comprises the following steps:

[0090] 10 g of 1,6-hexanediamine and 36 g of p-toluenesulfonyl isocyanate were added to 500 g of N,N-dimethylformamide, and the mixture was stirred at 35°C for 60 minutes. The product was separated to obtain a nucleating agent.

[0091] Preparation Example 2

[0092] The preparation method of modified polylactic acid-1 comprises the following steps:

[0093] 0.08 g of nucleating agent and 10 g of polylactic acid were mixed and added into an internal mixer. The temperature was adjusted to 180° C. and the rotation speed was 60 r / min. Melt blending was performed for 8 minutes, and then extrusion granulation was performed to obtain modified polylactic acid-1.

[0094] The nucleating agent is obtained from Preparation Example 1.

[0095] Preparation Example 3

[0096] The preparation method of modified polylactic acid-2 is the same as that of Preparation Example 2, except that the nucleating agent is replaced by a nucleating agent of the same mass, diphenyl dihydrazide sebacic acid SDA356.

[0097] Preparation Example 4

[0098] The preparation method of modified cellulose-1 comprises the following steps:

[0099] 0.8 g of polyvinyl alcohol was dissolved in 10 g of water, and 10 g of nanocellulose was dissolved in 100 g of N, N-dimethylacetamide. The solutions were then combined and stirred for 9 minutes to mix evenly. Under vacuum, the solution was irradiated at a dose of 3 KGy. The solvent was removed and the solution was dried to obtain modified cellulose-1.

[0100] Preparation Example 5

[0101] The preparation method of modified cellulose-2 is the same as that of Preparation Example 4, except that the nanocellulose is replaced by cellulose of the same mass.

[0102] Example 1

[0103] A degradable cooling filter rod material comprises the following raw materials, measured by weight: 145 parts of modified polylactic acid, 145 parts of modified cellulose and 1.5 parts of epoxy linseed oil.

[0104] The degradable cooling filter rod material in this embodiment is prepared by the following steps:

[0105] The modified polylactic acid-1, modified cellulose-1 and epoxy linseed oil are uniformly mixed, extruded by a screw extruder at an extrusion temperature of 200°C, pelletized and dried after extrusion to obtain a degradable cooling filter rod material.

[0106] Example 2

[0107] A degradable cooling filter rod material comprises the following raw materials, measured by weight: 130 parts of modified polylactic acid, 130 parts of modified cellulose and 1 part of epoxy linseed oil.

[0108] The degradable cooling filter rod material in this embodiment is prepared by the following steps:

[0109] The modified polylactic acid-1, modified cellulose-1 and epoxy linseed oil are uniformly mixed, extruded by a screw extruder at an extrusion temperature of 180°C, pelletized and dried after extrusion to obtain a degradable cooling filter rod material.

[0110] Example 3

[0111] A degradable cooling filter rod material comprises the following raw materials, measured by weight: 160 parts of modified polylactic acid, 160 parts of modified cellulose and 2 parts of epoxy linseed oil.

[0112] The degradable cooling filter rod material in this embodiment is prepared by the following steps:

[0113] The modified polylactic acid-1, modified cellulose-1 and epoxy linseed oil are uniformly mixed, extruded by a screw extruder at an extrusion temperature of 220°C, pelletized and dried after extrusion to obtain a degradable cooling filter rod material.

[0114] Example 4

[0115] This embodiment provides a degradable cooling filter rod material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified polylactic acid-1 is replaced by the same mass portion of modified polylactic acid-2.

[0116] Example 5

[0117] This embodiment provides a degradable cooling filter rod material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that the modified cellulose-1 is replaced by the same mass portion of modified cellulose-2.

[0118] Comparative Example 1

[0119] This comparative example provides a degradable cooling filter rod material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified polylactic acid-1 is replaced by polylactic acid of the same mass.

[0120] Comparative Example 2

[0121] This comparative example provides a degradable cooling filter rod material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the modified cellulose-1 is replaced by an equal mass portion of nanocellulose.

[0122] Performance Test:

[0123] 1. Heat resistance

[0124] The glass transition temperature and thermal decomposition temperature of the filter rod materials of the embodiments and comparative examples were determined by differential scanning calorimetry and thermogravimetric analysis.

[0125] 2. Mechanical properties

[0126] The elongation at break and impact strength of the filter rod materials of Examples 1-5 and Comparative Examples 1-2 were measured by a tensile testing machine and a cantilever beam impact testing machine. The tensile performance test was measured in accordance with the standard of GB / T1040.2-2006, and the impact performance test was measured in accordance with the standard of GB / T1843-2006. The results were taken as the average value of 5 test specimens.

[0127] 3. Cooling performance

[0128] The filter rod materials prepared in the examples and comparative examples were used in cigarettes, and smoking was simulated according to the cigarette smoking mode specified in the national standard YC / T29-1996. A K-type thermocouple temperature detector was used to detect the temperature at the center of the cigarette filter rod 2 mm away from the mouth end when the cigarette was smoked. The number of simulated smoking was 9 times, with an interval of 30 seconds between each puff, and the highest temperature was recorded.

[0129] The test results are shown in Table 1.

[0130] Table 1

[0131]

[0132] By comparing the experimental data of Examples 1-3 in Table 1, it can be seen that changing the ratio between the raw materials of the filter rod material still has good heat resistance, mechanical properties and cooling performance; by comparing Example 1 and Example 4, it can be seen that the modified polylactic acid-1 is replaced by the same mass of modified polylactic acid-2, and the nucleating agent is changed, resulting in a change in the crystallinity of polylactic acid, resulting in a slight decrease in the heat resistance and mechanical properties of the filter rod material; by comparing Example 1 and Example 5, it can be seen that the modified cellulose-1 is replaced by the same mass of modified cellulose-2, and the nanocellulose has a small particle size and a high specific The filter rod material prepared after modification has the characteristics of high surface area, high solubility and processability, and has higher heat resistance, mechanical properties and cooling performance; after comparing Example 1 with Comparative Example 1, it can be seen that the modified polylactic acid-1 is replaced by the same mass of polylactic acid. Due to the low glass transition temperature of polylactic acid, it is easy to soften when heated, resulting in a decrease in the heat resistance and mechanical properties of the filter rod material; after comparing Example 1 with Comparative Example 2, it can be seen that the modified cellulose-1 is replaced by the same mass of nanocellulose. Due to the poor compatibility between cellulose and polylactic acid, the mechanical properties of the filter rod material are reduced.

[0133] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A degradable cooling filter rod material, characterized in that: The invention comprises the following raw materials in parts by weight: 30-60 parts of modified polylactic acid, 30-60 parts of modified cellulose and 1-2 parts of stabilizer.

2. The cooling filter rod material according to claim 1, characterized in that: The preparation method of the modified polylactic acid comprises: The nucleating agent and polylactic acid are mixed and kneaded, and extruded and granulated to obtain modified polylactic acid; The temperature of the banburying is 170-190°C, the speed of the banburying is 55-65r / min, and the time of the banburying is 5-10min; The mass ratio of the polylactic acid to the nucleating agent is 1:(0.005-0.01).

3. The cooling filter rod material according to claim 2, characterized in that: The nucleating agent is shown in formula (I):

4. The cooling filter rod material according to claim 3, characterized in that: The preparation method of the nucleating agent comprises: Add 1,6-hexanediamine and p-toluenesulfonyl isocyanate to N,N-dimethylformamide, stir to react, and separate to obtain; The reaction temperature is 30-40°C, and the stirring time is 55-65min; The mass ratio of the 1,6-hexanediamine to p-toluenesulfonyl isocyanate is 1:(3.4-3.7).

5. The cooling filter rod material according to claim 1, characterized in that: The preparation of the modified cellulose comprises: The cellulose is dissolved in a solvent, mixed with a polyvinyl alcohol aqueous solution, stirred, vacuum irradiated, and dried to obtain the cellulose; the solvent includes N,N-dimethylacetamide; The stirring time is 8 to 10 minutes.

6. The cooling filter rod material according to claim 5, characterized in that: The mass ratio of the polyvinyl alcohol to the cellulose is (0.05-0.15):1; The vacuum degree of the vacuum irradiation is 0.08-0.1MPa; the irradiation source is an electron accelerator, and the irradiation dose is 1-5KGy.

7. The cooling filter rod material according to claim 1, characterized in that: The stabilizer is selected from any one of epoxidized linseed oil and epoxidized soybean oil.

8. A method for preparing a cooling filter rod material, characterized in that: The steps include: The modified polylactic acid, modified cellulose and stabilizer are uniformly mixed, extruded, pelletized and dried to obtain the product.

9. A cigarette filter rod, characterized in that: The raw material comprises the degradable cooling filter rod material according to any one of claims 1 to 7.

10. A cigarette, characterized in that: The cigarette filter rod comprises the cigarette filter rod as claimed in claim 9.