Environment-friendly corrosion-resistant coating material for wind power blade
By using environmentally friendly anti-corrosion coating materials on wind turbine blades, combined with atom transfer radical polymerization and ultrasonic-assisted preparation technology, the problem of traditional coating materials being harmful to the environment and human body is solved, and the durability and wear resistance of the coating are improved. properties, extending the service life of the blades.
Patent Information
- Application Number
- CN202411037072.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-18
AI Technical Summary
Traditional wind turbine blade coating materials contain volatile organic compounds, which are harmful to the environment and human body, and are easy to peel and fall off in harsh environments, resulting in poor corrosion resistance, resulting in reduced blade performance and shortened service life.
An environmentally friendly anti-corrosion coating material is used, including polymers, fillers, additives, pigments, solvents and environmentally friendly additives. The acrylic resin is prepared through atom transfer free radical polymerization, and glass beads are prepared through ultrasound-assisted preparation to improve the coating. Excellent adhesion, weather resistance, abrasion resistance and UV resistance.
It achieves the stability and durability of the coating in harsh environments, extends the service life of wind turbine blades, improves the corrosion resistance and wear resistance of the coating, and meets environmental protection requirements.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of anti-corrosion coatings, and in particular to an environmentally friendly anti-corrosion coating material for wind turbine blades. Background Art
[0002] Wind turbine blades are the core components of wind turbine generators. Their surfaces are often exposed to harsh natural environments, such as high temperature, high humidity, and ultraviolet rays. They are easily affected by oxidation, corrosion, and wear in the atmosphere, which leads to decreased blade performance and shortened life. In order to extend the service life of wind turbine blades and improve power generation efficiency, the blade surface needs to be protected. Traditional anti-corrosion coatings usually contain harmful volatile organic compounds, which are harmful to the environment and human body.
[0003] Environmentally friendly anti-corrosion coating materials for wind turbine blades have become one of the hot topics in current research. This coating material must not only have excellent corrosion resistance, wear resistance, and weather resistance, but also meet environmental protection requirements, that is, it is harmless to the environment and human body during the entire life cycle of coating, use, and disposal. The use of environmentally friendly anti-corrosion coating materials can reduce pollution to the environment, reduce production costs, and improve the sustainability and application value of the coating.
[0004] Traditional coating materials usually contain volatile organic compounds, which are easy to evaporate and release harmful substances, causing harm to the environment and human body. They are easy to peel and fall off in harsh environments such as high temperature, high humidity, and ultraviolet rays, causing coating failure. In particular, they have poor corrosion resistance and are easily affected by oxidation, corrosion, and wear in the atmosphere, resulting in reduced blade performance and shortened life. Summary of the invention
[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose an environmentally friendly anti-corrosion coating material for wind turbine blades.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] An environmentally friendly anti-corrosion coating material for wind turbine blades, comprising a polymer, a filler, an additive, a pigment, a solvent and an environmentally friendly additive, the quality ratio of which is as follows:
[0008] Polymer 52%-75%;
[0009] Filler 12%-34%;
[0010] Additives 6%-14%;
[0011] Pigment 4%-9%;
[0012] Solvent 5%-15%;
[0013] Environmentally friendly additives 7%-9%.
[0014] Preferably, the polymer and filler have the following specific components:
[0015] Polymers include epoxies, polyurethanes, acrylics, silicones, polyimides, and polypropylene;
[0016] Fillers include alumina, glass beads and calcium carbonate.
[0017] Furthermore: the auxiliary agent is selected from any two or more of polyisocyanate, colloidal silica, bentonite, organotin, aluminum hydroxide and ammonium phosphate, the pigment is selected from any two or more of zinc oxide, sodium tripolyphosphate and titanium dioxide, the solvent is selected from any one or more of ethanol, acetone and xylene, and the environmentally friendly additive is selected from any two or more of linseed oil, acrylic emulsion and citric acid.
[0018] On the basis of the above scheme: the mass composition of the polymer, filler, additive, pigment, solvent and environmentally friendly additive is as follows:
[0019] 30-40 parts of epoxy resin, 12-22 parts of polyurethane, 10-20 parts of acrylic resin, 7-9 parts of silicone resin, 5-7 parts of polyimide, 4-8 parts of polypropylene, 6-10 parts of aluminum oxide, 8-13 parts of glass beads, 6-15 parts of calcium carbonate, 3-5 parts of polyisocyanate, 1-3 parts of colloidal silica, 2-4 parts of bentonite, 1-3 parts of organotin, 1-2 parts of aluminum hydroxide, 1-3 parts of ammonium phosphate, 2-3 parts of zinc oxide, 4-5 parts of sodium tripolyphosphate, 1-3 parts of titanium dioxide, 5-15 parts of ethanol, 4-17 parts of acetone, 10-12 parts of xylene, 7-10 parts of linseed oil, 6-8 parts of acrylic emulsion, and 4-6 parts of citric acid.
[0020] A more preferred solution in the above solution is that the acrylic resin in the polymer is prepared by the following method:
[0021] A1: prepare acrylic acid monomer, acrylic acid ester monomer, copper ion and acetylacetone;
[0022] A2: introducing the raw materials into a reaction kettle containing argon;
[0023] A3: copper ions and acetylacetone are added to the reactor, and the polymerization reaction begins under the action of copper ions and acetylacetone;
[0024] A4: After the polymerization reaction is completed, the product is distilled, crystallized and filtered to obtain a pure acrylic resin product.
[0025] As a further solution of the present invention: the pressure in the reactor is controlled to be 101-123 kPa and the temperature is 45-86°C.
[0026] Meanwhile, the glass microbeads in the filler are prepared in the following specific steps:
[0027] B1: Boric acid is selected as a glass raw material, and it is crushed and screened to obtain glass powder;
[0028] B2: mixing glass powder and water to obtain a glass solution;
[0029] B3: Pour the glass solution into the reaction container and insert the ultrasonic transducer into the solution;
[0030] B4: Start the ultrasonic generator to generate strong mechanical vibrations in the solution. The energy of the ultrasonic wave will accelerate the condensation and nucleation of the glass solution, prompting the glass material to quickly form tiny particles.
[0031] B4: After stopping the ultrasonic vibration, the glass beads will settle to the bottom of the reaction container. The glass beads are separated by filtering, centrifuging, etc., and then washed and dried to obtain the desired glass beads.
[0032] As a preferred embodiment of the present invention, the particle size of the glass powder is 1-10 microns, and the ratio of glass powder to water is 1:5.
[0033] Meanwhile, the working time of the ultrasonic generator is 1-1.5h.
[0034] A method for preparing an environmentally friendly anti-corrosion coating material for wind turbine blades comprises the following steps: epoxy resin, polyurethane, acrylic resin, silicone resin, polyimide, polypropylene, aluminum oxide, glass microbeads, calcium carbonate, polyisocyanate, colloidal silicon, bentonite, organic tin, aluminum hydroxide, ammonium phosphate, zinc oxide, sodium tripolyphosphate, titanium dioxide, ethanol, acetone, xylene, linseed oil, acrylic emulsion and citric acid are weighed and then mixed, and dispersed, ground and filtered to obtain the coating material.
[0035] The beneficial effects of the present invention are:
[0036] 1. An environmentally friendly anti-corrosion coating material for wind turbine blades, epoxy resin, polyurethane, acrylic resin and silicone resin provide the coating with adhesion, flexibility and weather resistance, and epoxy resin is used as the main matrix, and a small amount of polyurethane is added to improve flexibility, or acrylic resin is used as the matrix, and silicone resin is added to improve heat resistance and chemical resistance; aluminum oxide, glass beads and calcium carbonate improve the hardness, wear resistance and corrosion resistance of the coating, increase the density and reduce the thickness of the coating; polyisocyanate, colloidal silicon and bentonite can improve the adhesion, waterproofness and UV resistance of the coating, and organic tin, aluminum hydroxide, ammonium phosphate, zinc oxide and sodium tripolyphosphate can improve the corrosion resistance, heat resistance and chemical resistance of the coating.
[0037] 2. This environmentally friendly anti-corrosion coating material for wind turbine blades uses an atom transfer radical polymerization method to prepare acrylic resin for use in environmentally friendly anti-corrosion coating materials for wind turbine blades. It can achieve precise control of the molecular weight and molecular weight distribution of the polymer, so that an acrylic resin with a specific molecular structure and molecular weight can be prepared, which is beneficial to regulating the performance of the coating. The prepared high-molecular-weight acrylic resin can provide better performance for the coating material, such as better corrosion resistance and weather resistance. At the same time, the prepared high-molecular-weight acrylic resin has a narrow molecular weight distribution, and a more uniform product can be obtained, thereby improving the quality and stability of the coating and being more in line with environmental protection requirements. The polymerization reaction rate and molecular weight distribution are highly controllable and can be adjusted according to specific needs and application requirements to meet the coating performance requirements in different scenarios.
[0038] 3. This kind of environmentally friendly anti-corrosion coating material for wind turbine blades, in the preparation of the environmentally friendly anti-corrosion coating material for wind turbine blades, uses glass microbeads prepared with the assistance of ultrasound to improve the durability and wear resistance of the wind turbine blade surface; at the same time, it improves the adhesion between the coating and the substrate, prevents the coating from peeling and falling off, and ensures the stability of the coating in harsh environments; improves the gloss and appearance of the coating. Glass microbeads have good chemical stability. Adding them to the coating can improve the corrosion resistance of the coating and enhance the resistance of wind turbine blades to corrosive media. It can improve the performance and stability of the coating and extend the service life of the coating. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.
[0040] An environmentally friendly anti-corrosion coating material for wind turbine blades, comprising a polymer, a filler, an additive, a pigment, a solvent and an environmentally friendly additive, the quality ratio of which is as follows:
[0041] Polymer 52%-75%;
[0042] Filler 12%-34%;
[0043] Additives 6%-14%;
[0044] Pigment 4%-9%;
[0045] Solvent 5%-15%;
[0046] Environmentally friendly additives 7%-9%.
[0047] The specific ingredients of the polymer, filler, additive, pigment, solvent and environmentally friendly additive are as follows:
[0048] Polymers include epoxies, polyurethanes, acrylics, silicones, polyimides, and polypropylene;
[0049] Fillers include alumina, glass beads, and calcium carbonate;
[0050] The auxiliary agent includes any two or more of polyisocyanate, colloidal silica, bentonite, organotin, aluminum hydroxide and ammonium phosphate;
[0051] The pigment includes any two or more of zinc oxide, sodium tripolyphosphate and titanium dioxide;
[0052] The solvent includes any one or more of ethanol, acetone and xylene;
[0053] The environmentally friendly additives include any two or more of linseed oil, acrylic emulsion and citric acid.
[0054] The polymer, filler, additive, pigment, solvent and environmentally friendly additive have the following mass components:
[0055] 30-40 parts of epoxy resin, 12-22 parts of polyurethane, 10-20 parts of acrylic resin, 7-9 parts of silicone resin, 5-7 parts of polyimide, 4-8 parts of polypropylene, 6-10 parts of aluminum oxide, 8-13 parts of glass beads, 6-15 parts of calcium carbonate, 3-5 parts of polyisocyanate, 1-3 parts of colloidal silica, 2-4 parts of bentonite, 1-3 parts of organotin, 1-2 parts of aluminum hydroxide, 1-3 parts of ammonium phosphate, 2-3 parts of zinc oxide, 4-5 parts of sodium tripolyphosphate, 1-3 parts of titanium dioxide, 5-15 parts of ethanol, 4-17 parts of acetone, 10-12 parts of xylene, 7-10 parts of linseed oil, 6-8 parts of acrylic emulsion, and 4-6 parts of citric acid.
[0056] The coating materials involved in the following embodiments are prepared by the following preparation method:
[0057] Epoxy resin, polyurethane, acrylic resin, silicone resin, polyimide, polypropylene, aluminum oxide, glass microbeads, calcium carbonate, polyisocyanate, colloidal silicon, bentonite, organotin, aluminum hydroxide, ammonium phosphate, zinc oxide, sodium tripolyphosphate, titanium dioxide, ethanol, acetone, xylene, linseed oil, acrylic emulsion and citric acid are weighed and mixed, and then dispersed, ground and filtered to obtain the coating material.
[0058] The acrylic resin involved in the invention has the following preparation method:
[0059] A1: Prepare 10%-50% acrylic acid monomer, 12%-45% acrylate monomer, 0.2%-4% copper ion and 0.5%-8% acetylacetone;
[0060] A2: Introduce the raw materials into a reactor containing 90% argon, and control the pressure of the reactor to 101-123 kPa and the temperature to 45-86°C;
[0061] A3: copper ions and acetylacetone are added to the reactor in an isochronous intermittent manner, and a polymerization reaction is initiated under the action of copper ions and acetylacetone;
[0062] A4: After the polymerization reaction is completed, the product is distilled, crystallized and filtered to obtain a pure acrylic resin product.
[0063] The atom transfer radical polymerization method is used to prepare acrylic resin for use in environmentally friendly anti-corrosion coating materials for wind turbine blades. It is possible to achieve precise control of the polymer molecular weight and molecular weight distribution, so that acrylic resin with a specific molecular structure and molecular weight can be prepared, which is beneficial to regulating the performance of the coating. The prepared high molecular weight acrylic resin can provide better performance of the coating material, such as better corrosion resistance and weather resistance. At the same time, the prepared high molecular weight acrylic resin has a narrow molecular weight distribution, which can obtain a more uniform product, improve the quality and stability of the coating, and better meet environmental protection requirements. Among them, the polymerization reaction rate and molecular weight distribution are highly controllable and can be adjusted according to specific needs and application requirements to meet the coating performance requirements in different scenarios.
[0064] The glass microbeads involved in the coating material are prepared by ultrasound assistance, and the specific steps are as follows:
[0065] B1: Boric acid is selected as the glass raw material, and it is crushed and screened to obtain glass powder with a particle size of 1-10 microns;
[0066] B2: Mix glass powder and water in a ratio of 1:5 and stir to obtain a glass solution;
[0067] B3: Pour the glass solution into the reaction container and insert the ultrasonic transducer into the solution;
[0068] B4: Start the ultrasonic generator to generate strong mechanical vibration in the solution. The energy of the ultrasonic wave will accelerate the condensation and nucleation of the glass solution, prompting the glass material to quickly form tiny particles. The control time is 1-1.5h;
[0069] B4: After stopping the ultrasonic vibration, the glass beads will settle to the bottom of the reaction container. The glass beads are separated by filtering, centrifuging, etc., and then washed and dried to obtain the desired glass beads.
[0070] In the preparation of environmentally friendly anti-corrosion coating materials for wind turbine blades, glass microbeads prepared with the assistance of ultrasound can improve the durability and wear resistance of the wind turbine blade surface; at the same time, the adhesion between the coating and the substrate is improved, the coating is prevented from peeling and falling off, and the stability of the coating in harsh environments is ensured; the gloss and appearance of the coating are improved. Glass microbeads have good chemical stability. Adding them to the coating can improve the corrosion resistance of the coating and enhance the resistance of wind turbine blades to corrosive media. It can improve the performance and stability of the coating and extend the service life of the coating.
[0071] Embodiment 1:
[0072] An environmentally friendly anti-corrosion coating material for wind turbine blades, the polymer, filler, auxiliary agent, pigment, solvent and environmentally friendly additive, the mass composition of which is as follows:
[0073] 32 parts of epoxy resin, 14 parts of polyurethane, 17 parts of acrylic resin, 8 parts of silicone resin, 6 parts of polyimide, 5 parts of polypropylene, 6 parts of aluminum oxide, 9 parts of glass microspheres, 11 parts of calcium carbonate, 3 parts of bentonite, 1 part of organic tin, 2 parts of aluminum hydroxide, 3 parts of ammonium phosphate, 2 parts of sodium tripolyphosphate, 2 parts of titanium dioxide, 12 parts of ethanol, 8 parts of linseed oil, and 7 parts of acrylic emulsion.
[0074] Embodiment 2:
[0075] An environmentally friendly anti-corrosion coating material for wind turbine blades, the polymer, filler, auxiliary agent, pigment, solvent and environmentally friendly additive, the mass composition of which is as follows:
[0076] 30 parts of epoxy resin, 12 parts of polyurethane, 14 parts of acrylic resin, 9 parts of silicone resin, 7 parts of polyimide, 7 parts of polypropylene, 6 parts of aluminum oxide, 12 parts of glass beads, 10 parts of calcium carbonate, 5 parts of polyisocyanate, 3 parts of colloidal silicon, 1 part of aluminum hydroxide, 2 parts of ammonium phosphate, 2 parts of zinc oxide, 4 parts of sodium tripolyphosphate, 3 parts of titanium dioxide, 11 parts of ethanol, 7 parts of linseed oil, and 8 parts of acrylic emulsion.
[0077] Embodiment 3:
[0078] An environmentally friendly anti-corrosion coating material for wind turbine blades, the polymer, filler, auxiliary agent, pigment, solvent and environmentally friendly additive, the mass composition of which is as follows:
[0079] 35 parts of epoxy resin, 15 parts of polyurethane, 15 parts of acrylic resin, 10 parts of silicone resin, 6 parts of polyimide, 6 parts of polypropylene, 8 parts of aluminum oxide, 12 parts of glass beads, 10 parts of calcium carbonate, 5 parts of polyisocyanate, 3 parts of colloidal silicon, 1 part of aluminum hydroxide, 2 parts of ammonium phosphate, 2 parts of zinc oxide, 4 parts of sodium tripolyphosphate, 3 parts of titanium dioxide, 11 parts of xylene, 7 parts of linseed oil, 8 parts of acrylic emulsion, and 5 parts of citric acid.
[0080] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. An environmentally friendly anti-corrosion coating material for wind turbine blades, comprising a polymer, a filler, an additive, a pigment, a solvent and an environmentally friendly additive, It is characterized in that The quality ratio is as follows: Polymer 52%-75%; Filler 12%-34%; Additives 6%-14%; Pigment 4%-9%; Solvent 5%-15%; Environmentally friendly additives 7%-9%.
2. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 1, It is characterized in that The specific ingredients of the polymer and filler are as follows: Polymers include epoxies, polyurethanes, acrylics, silicones, polyimides, and polypropylene; Fillers include alumina, glass beads and calcium carbonate.
3. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 1, It is characterized in that The auxiliary agent is selected from any two or more of polyisocyanate, colloidal silica, bentonite, organotin, aluminum hydroxide and ammonium phosphate; the pigment is selected from any two or more of zinc oxide, sodium tripolyphosphate and titanium dioxide; the solvent is selected from any one or more of ethanol, acetone and xylene; and the environmentally friendly additive is selected from any two or more of linseed oil, acrylic emulsion and citric acid.
4. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 3, It is characterized in that The polymer, filler, additive, pigment, solvent and environmentally friendly additive have the following mass components: 30-40 parts of epoxy resin, 12-22 parts of polyurethane, 10-20 parts of acrylic resin, 7-9 parts of silicone resin, 5-7 parts of polyimide, 4-8 parts of polypropylene, 6-10 parts of aluminum oxide, 8-13 parts of glass beads, 6-15 parts of calcium carbonate, 3-5 parts of polyisocyanate, 1-3 parts of colloidal silica, 2-4 parts of bentonite, 1-3 parts of organotin, 1-2 parts of aluminum hydroxide, 1-3 parts of ammonium phosphate, 2-3 parts of zinc oxide, 4-5 parts of sodium tripolyphosphate, 1-3 parts of titanium dioxide, 5-15 parts of ethanol, 4-17 parts of acetone, 10-12 parts of xylene, 7-10 parts of linseed oil, 6-8 parts of acrylic emulsion, and 4-6 parts of citric acid.
5. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 4, It is characterized in that The acrylic resin in the polymer is prepared by the following method: A1: prepare acrylic acid monomer, acrylic acid ester monomer, copper ion and acetylacetone; A2: introducing the raw materials into a reaction kettle containing argon; A3: copper ions and acetylacetone are added to the reactor, and polymerization reaction is initiated under the action of copper ions and acetylacetone; A4: After the polymerization reaction is completed, the product is distilled, crystallized and filtered to obtain a pure acrylic resin product.
6. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 5, It is characterized in that The pressure in the reactor is controlled at 101-123 kPa and the temperature is controlled at 45-86°C.
7. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 1, It is characterized in that The glass microspheres in the filler are prepared in the following specific steps: B1: Boric acid is selected as a glass raw material, and it is crushed and screened to obtain glass powder; B2: mixing glass powder and water to obtain a glass solution; B3: Pour the glass solution into the reaction container and insert the ultrasonic transducer into the solution; B4: Start the ultrasonic generator to generate strong mechanical vibrations in the solution. The energy of the ultrasonic wave will accelerate the condensation and nucleation of the glass solution, prompting the glass material to quickly form tiny particles. B4: After stopping the ultrasonic vibration, the glass beads will settle to the bottom of the reaction container. The glass beads are separated by filtering, centrifuging, etc., and then washed and dried to obtain the desired glass beads.
8. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 7, It is characterized in that The particle size of the glass powder is 1-10 microns, and the ratio of the glass powder to water is 1:
5.
9. The environmentally friendly anti-corrosion coating material for wind turbine blades according to claim 7, It is characterized in that The working time of the ultrasonic generator is 1-1.5h.
10. A method for preparing an environmentally friendly anti-corrosion coating material for a wind turbine blade according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Epoxy resin, polyurethane, acrylic resin, silicone resin, polyimide, polypropylene, aluminum oxide, glass microbeads, calcium carbonate, polyisocyanate, colloidal silicon, bentonite, organotin, aluminum hydroxide, ammonium phosphate, zinc oxide, sodium tripolyphosphate, titanium dioxide, ethanol, acetone, xylene, linseed oil, acrylic emulsion and citric acid are weighed and mixed, and then dispersed, ground and filtered to obtain the coating material.