High-performance epoxy filling and repairing adhesive and preparation method thereof

By combining the use of bisphenol A and F epoxy resins and specific fillers, a high-performance epoxy filled repair adhesive is prepared, which solves the problems of slow adhesive curing speed and insufficient bonding strength in EMU floor installation, and achieves high efficiency Bonding and repair effects.

CN118792002APending Publication Date: 2024-10-18KUNSHAN AICA KOGYO CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411016311.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-27
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Due to problems such as slow curing speed, insufficient bonding strength, and large curing shrinkage during the installation process of EMU floors, existing adhesives are difficult to meet the bonding and repair needs of various floor materials.

Method used

Bisphenol A and F epoxy resins are combined, epoxy silane modified heavy calcium carbonate and stearic acid modified calcium carbonate are added, together with polyamide curing agent and silane coupling agent, through a specific mixing process and composition. According to the proportion, a high-performance epoxy filled repair adhesive is prepared to improve the bonding strength, hardness and curing speed.

Benefits of technology

It achieves an adhesive with fast curing, high bonding strength, high hardness and low shrinkage. It is suitable for bonding and repairing a variety of base materials, simplifying the construction process and improving construction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965796880000111
    Figure BDA0004965796880000111
  • Figure BDA0004965796880000121
    Figure BDA0004965796880000121
Patent Text Reader

Abstract

The invention relates to a high-performance epoxy filling and repairing adhesive and a preparation method thereof.The high-performance epoxy filling and repairing adhesive is prepared from, by weight, an agent A and an agent B. The agent A is prepared from bisphenol A type epoxy resin, bisphenol F type epoxy resin, ground calcium carbonate, surface treatment calcium carbonate, titanium dioxide, a thixotropic agent, color paste and a reactive diluent; the agent B is prepared from the following raw materials: a polyamide curing agent, heavy calcium carbonate, surface treatment calcium carbonate, titanium dioxide, a thixotropic agent, color paste powder, a curing accelerator, a silane coupling agent and a fatty amine curing agent. The high-performance epoxy filling and repairing adhesive disclosed by the invention is high in bonding strength, high in hardness, fast in curing and suitable for filling and repairing various materials, especially for filling and repairing floors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an adhesive, and more specifically, to a high-performance epoxy-filled repair adhesive and a preparation method thereof. Background Art

[0002] The interior decoration of the EMU is a factor that directly affects the beauty of the EMU, and the floor is a key component of the interior decoration of the EMU. Due to the long-term flow of people during operation, the overall structure of the floor or its own expansion and contraction will cause changes in the joints of the floor, resulting in deformation of the floor. Therefore, the adhesive must have higher bonding strength, hardness, toughness, and lower curing shrinkage to avoid defects in the floor and floor cloth caused by deformation of the substrate structure. The prior art generally increases the hardness of the adhesive by adding reinforcing fillers, but the reinforcing fillers are generally not compatible with the adhesive, and are prone to agglomeration or precipitation, affecting the strength and bonding effect of the adhesive. In addition, during the installation of the floor, due to the problem of slow curing speed, personnel will not be able to perform other work on the floor in time. Therefore, there are certain requirements for the curing speed of the adhesive.

[0003] How to provide an adhesive with fast curing, high bonding strength, high hardness, low curing shrinkage, affinity to the bonded materials, and able to meet the bonding and repair needs of various materials such as flooring is a problem to be solved. Summary of the invention

[0004] In order to solve the problem of adhesives, the present application provides a high-performance epoxy-filled repair adhesive and a preparation method thereof.

[0005] In the first aspect, the present application provides a high-performance epoxy filling repair adhesive, comprising agent A and agent B, wherein agent A comprises the following raw materials in parts by mass: 30-35 parts of bisphenol A epoxy resin, 5-10 parts of bisphenol F epoxy resin, 30-40 parts of heavy calcium carbonate, 15-20 parts of surface-treated calcium carbonate, 1-3 parts of titanium dioxide, 1-3 parts of thixotropic agent, 0.01 parts of color paste, and 6.5-8.5 parts of active diluent; agent B comprises the following raw materials in parts by mass: 20-24 parts of polyamide curing agent, 30-40 parts of heavy calcium carbonate, 15-20 parts of surface-treated calcium carbonate, 1-3 parts of titanium dioxide, 1-3 parts of thixotropic agent, 0.01-0.02 parts of color paste, 1-3 parts of curing accelerator, 1-2 parts of silane coupling agent, and 20-24 parts of fatty amine curing agent.

[0006] By adopting the above scheme, the raw materials of bisphenol A epoxy resin are easy to obtain and low in cost. It basically does not produce small molecular volatiles during curing. The cured product has high bonding strength and hardness, and also has certain toughness. Bisphenol F epoxy resin has good impregnation property for the bonding substrate and high bonding strength. By using bisphenol A epoxy resin and bisphenol F epoxy resin together at a certain mass ratio, the prepared adhesive can penetrate into the gaps of the bonding surface to achieve full infiltration, good bonding effect, less bubbles in the adhesive layer, and less likely to shrink after curing. Heavy calcium carbonate has less water content and greater bulk density. By adding a certain mass of heavy calcium carbonate to the adhesive, the hardness of the adhesive is increased and the shrinkage is reduced. Due to the irregular shape of heavy calcium carbonate particles, it is not easy to flow in the adhesive and is not easy to deposit during the curing process, so the prepared adhesive is more uniform. By adding surface treated calcium carbonate, the compatibility of calcium carbonate with the adhesive is good, and the dispersibility and stability of calcium carbonate in the adhesive are better, which further improves the bonding strength of the adhesive, and the obtained adhesive is flexible and not easy to shrink after curing. By adding a certain amount of thixotropic agent, the adhesive is provided with thixotropic rheology, which further makes the components of the adhesive less likely to precipitate, and the obtained adhesive is more uniform. By adding active diluent, the wettability of the adhesive on non-polar surfaces is improved, and the obtained adhesive has higher bonding strength and flexibility. By adding a certain amount of polyamide curing agent and modified fatty amine curing agent for combined curing, the curing speed is fast, which effectively solves the problem of slow construction progress. By adding a certain amount of curing accelerator, the curing efficiency of polyamide curing agent and modified fatty amine curing agent is further improved. By adding silane coupling agent, the affinity and moisture and heat resistance of epoxy resin adhesive to the bonded material are improved, and the bonding strength is further improved to meet the bonding and repair needs of various materials. By adding color paste to agent A and agent B, it is easy to distinguish agent A and agent B. By adding titanium dioxide, the coloring power of the color paste is increased and the amount of color paste added is reduced.

[0007] In a specific embodiment, the heavy calcium carbonate is epoxysilane-modified heavy calcium carbonate, and the surface-treated calcium carbonate is stearic acid-modified light calcium carbonate.

[0008] By adopting the above scheme, epoxysilane-modified heavy calcium carbonate has better dispersibility in the adhesive, and at the same time, the content of epoxy groups is increased to further improve the adhesive bonding strength. Some epoxy groups participate in curing, further improving the cross-linking strength of the adhesive. By adding stearic acid to modify calcium carbonate, stearate is adsorbed on the surface of calcium carbonate, the surface energy is reduced, it is not easy to agglomerate, and it has good compatibility with the adhesive. It is better dispersed in the adhesive and also shows good thixotropy, further improving the adhesive strength.

[0009] In a specific embodiment, in Agent A and Agent B: the mesh size of heavy calcium carbonate is 800-1000 mesh, and the mesh size of light calcium carbonate is 2000-2500 mesh.

[0010] By adopting the above scheme, the mesh number of heavy calcium carbonate is limited to 800-1000 mesh, thereby further improving the hardness of the adhesive, and the mesh number of surface-treated calcium carbonate is limited to 2000-2500 mesh, thereby further improving the thixotropy and bonding strength of the adhesive, and by using two mesh numbers of calcium carbonate together, the calcium carbonate is evenly distributed and filled in the adhesive, thereby further eliminating the internal defects of the adhesive, and the obtained adhesive has a small volume shrinkage after curing. At the same time, the combination of calcium carbonates of different mesh numbers reduces the added mass of calcium carbonate, thereby further improving the bonding strength of the adhesive.

[0011] In a specific embodiment, the amine value of the polyamide curing agent is 150-220 mg KOH / g.

[0012] By adopting the above scheme and limiting the amine value of the polyamide curing agent, the viscosity of the curing agent is high, which further improves the bonding strength of the adhesive and is suitable for the bonding and filling of the adhesive in this application.

[0013] In a specific embodiment, the polyamide curing agent includes a polyamide curing agent with a weight average molecular weight of 500-1000g / mol and a polyamide curing agent with a weight average molecular weight of 7000-9000g / mol. By adopting the above scheme, by adding the polyamide curing agent, the bonding performance of the adhesive and the adhesion to the substrate are further improved. The polyamide curing agent can be cured at room temperature, is easy to operate, and has a fast curing speed, which further simplifies the operation of the adhesive. By adding a polyamide curing agent with a lower molecular weight, the polyamide curing agent has excellent bonding performance. After curing, the molecules intersperse with each other, and the obtained adhesive has better toughness and greater bonding strength.

[0014] In a specific embodiment, the reactive diluent comprises a C12-14 alkyl glycidyl ether.

[0015] By adopting the above scheme, the prepared adhesive has good wettability to non-polar surfaces and good flexibility, and the bonding strength of the adhesive is further improved.

[0016] In a specific embodiment, the curing accelerator includes 2,4,6-tris(dimethylaminomethyl)phenol.

[0017] By adopting the above scheme, the promoting effect on the polyamide curing agent and the fatty amine curing agent is good, and the prepared adhesive cures quickly, has a good curing effect, has a uniform and stable structure, and has a high bonding strength.

[0018] In a specific embodiment, the silane coupling agent includes 3-glycidoxypropyltrimethoxysilane.

[0019] By adopting the above scheme, the affinity and moisture and heat resistance of the epoxy resin adhesive to the bonded material are improved, and other active groups in the silane coupling agent react with the epoxy resin or curing agent to increase the cross-linking polymerization ability of the glue, further improving the bonding strength of the adhesive.

[0020] In a second aspect, the present application provides a method for preparing a high-performance epoxy-filled repair adhesive, comprising the following steps: uniformly mixing agent A and agent B in a weight ratio of (1.9-2.2):1 to obtain a high-performance epoxy-filled repair adhesive.

[0021] By adopting the above technical solution, the adhesive cures quickly and fully, and the prepared adhesive has toughness, is not brittle, and has high bonding strength.

[0022] In a specific embodiment, the preparation method of agent A includes: S1. mixing part of bisphenol A epoxy resin, bisphenol F epoxy resin, heavy calcium carbonate, surface treated calcium carbonate, titanium dioxide, thixotropic agent and color paste, stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 20-40 minutes under vacuum; S2. adding active diluent and the remaining bisphenol A epoxy resin, stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 10-30 minutes under vacuum to obtain agent A; the preparation method of agent B includes: S1. mixing polyamide curing agent, heavy calcium carbonate, surface treated calcium carbonate, titanium dioxide, thixotropic agent and color paste, stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 20-40 minutes under vacuum; S2. adding curing accelerator, silane coupling agent and fatty amine curing agent, stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 10-30 minutes under vacuum to obtain agent B.

[0023] By adopting the above scheme, the components of the prepared A and B agents are uniform and stable, fewer bubbles enter the adhesive during stirring, the prepared A and B agents have a low curing shrinkage rate after mixing, and the prepared adhesive has higher hardness and bonding strength.

[0024] In summary, this application has the following beneficial effects: 1. Compared with the prior art, the adhesive prepared by the present application adopts bisphenol A and F type epoxy resins and cooperates with surface treated fillers, and has higher bonding strength, which is suitable for bonding of various substrates. It has high hardness and certain toughness, and it is not easy to produce marks after polishing. It has good initial adhesion and good workability. By using a certain quality of polyamide curing agent and fatty amine curing agent in conjunction with a curing accelerator, the curing speed is fast, and the construction time can be shortened. By using a curing agent in conjunction with a silane coupling agent, the affinity of the adhesive to the bonded material is increased, which can meet the bonding and repair requirements of various materials. By limiting the stirring time, stirring speed and order of adding raw materials during the preparation of Agent A and Agent B, the obtained adhesive is evenly mixed, free of bubbles, and has a low shrinkage rate after curing.

[0025] 2. This application adds a certain mass of epoxysilane-modified calcium carbonate and stearic acid-modified calcium carbonate, and limits the mesh size of the calcium carbonate to two different ranges. The filler is evenly distributed in the adhesive and does not sink to the bottom. By limiting the amine value and two different molecular weights of the polyamide curing agent, the obtained adhesive is uniform and flat, has a good curing effect, and has high bonding strength and hardness. DETAILED DESCRIPTION

[0026] In the preparation examples, embodiments, and comparative examples, heavy calcium carbonate and light calcium carbonate are all from Shanghai Liangjiang Chemical, polyamide curing agents are all from Kain Chemical Co., Ltd., thixotropic agents are all SDJ9931 from Sandingjia Co., Ltd., fatty amine curing agents are all H-55 from Chubu Chemical Co., Ltd., reactive diluents are all C12-14 alkyl glycidyl ethers, curing accelerators are all 2,4,6-tris(dimethylaminomethyl)phenol, silane coupling agents are all 3-glycidyloxypropyltrimethoxysilane, and other experimental reagents, unless otherwise specified, are all conventional commercial brands or obtained through conventional preparation processes.

[0027] Preparation Example Preparation Example 1 Epoxysilane modified heavy calcium carbonate 10 g of 800 mesh heavy calcium carbonate was added to 200 ml of toluene, and ultrasonic dispersion was performed at 300 W for 30 minutes to obtain a suspension. 0.5 g of epoxy silane coupling agent KH-560 was added to the mixed solution, ultrasonic dispersion was performed at 300 W for 5 minutes, and the mixture was filtered, reacted at 90 ° C for 6 hours, and then dried at 80 ° C for 6 hours to obtain epoxy silane modified silica.

[0028] Preparation Example 2 Stearic acid modified light calcium carbonate Add 5 g of 2000 mesh light calcium carbonate into 300 g of deionized water, stir for 30 minutes, then add 1000 ml of 1% stearic acid ethanol solution, pass nitrogen, stir at 1000 rpm for 30 minutes, centrifuge for 30 minutes, wash with ethanol 3 times, and dry to obtain stearic acid modified light calcium carbonate.

[0029] Preparation Example 3 The only difference between this preparation example and preparation example 1 is that the mesh number of the heavy calcium carbonate is 400 mesh.

[0030] Preparation Example 4 The only difference between this preparation example and preparation example 2 is that the mesh size of the light calcium carbonate is 5000 mesh.

[0031] Preparation Example 5 Stearic acid modified heavy calcium carbonate 5 g of 800 mesh heavy calcium carbonate was added into 300 g of deionized water and stirred for 30 minutes. Then 1000 ml of 1% stearic acid ethanol solution was added, nitrogen was introduced, stirred at 1000 rpm for 30 minutes, centrifuged for 30 minutes, washed with ethanol 3 times, and dried to obtain stearic acid modified heavy calcium carbonate. Example

[0032] Example 1 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 350 g of 800 mesh heavy calcium carbonate, 150 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight-average molecular weight of 700 g / mol, 350 g of 800 mesh heavy calcium carbonate, 150 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring tank and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0033] Example 2 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 100 g of bisphenol F epoxy resin, 350 g of 800 mesh heavy calcium carbonate, 150 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 15 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2. Add 65 g of active diluent and the remaining 100 g of bisphenol A epoxy resin to the intermediate product of Agent A, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 240 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight average molecular weight of 700 g / mol, 350 g of 800 mesh heavy calcium carbonate, 150 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring tank and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 200 g of fatty amine curing agent to the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0034] Example 3 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 300 g of 800 mesh heavy calcium carbonate, 200 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 15 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2. Add 85 g of active diluent and the remaining 130 g of bisphenol A epoxy resin to the intermediate product of Agent A, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min at a stirring speed of 1000 r / min under vacuum, filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 200g of a polyamide curing agent having an amine value of 200mg KOH / g and a weight-average molecular weight of 700g / mol, 350g of 800-mesh heavy calcium carbonate, 150g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20g of titanium dioxide, 20g of a thixotropic agent, and 0.1g of a green slurry were added to a stirring tank and stirred at a low speed for 10min at a stirring speed of 300r / min, and then stirred at a high speed for 30min under vacuum at a stirring speed of 1000r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 240 g of fatty amine curing agent to the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0035] Example 4 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 2, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight-average molecular weight of 700 g / mol, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 2, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring kettle and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0036] Example 5 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 3, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 2, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight-average molecular weight of 700 g / mol, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 3, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 2, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring kettle and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0037] Example 6 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 4, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight-average molecular weight of 700 g / mol, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 4, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring kettle and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0038] Example 7 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified heavy calcium carbonate prepared in Preparation Example 5, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an agent A intermediate; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight-average molecular weight of 700 g / mol, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified heavy calcium carbonate prepared in Preparation Example 5, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring kettle and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0039] Example 8 The only difference between this embodiment and embodiment 4 is that the amine value of the polyamide curing agent is 120 mg KOH / g.

[0040] Example 9 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 50 g of bisphenol F epoxy resin, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 2, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were added into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent A; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 110 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight average molecular weight of 700 g / mol, 110 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight average molecular weight of 8000 g / mol, 350 g of epoxysilane-modified heavy calcium carbonate prepared in Preparation Example 1, 150 g of stearic acid-modified light calcium carbonate prepared in Preparation Example 2, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring tank and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0041] Example 10 The only difference between this embodiment and embodiment 4 is that the molecular weight of the polyamide curing agent is 8000 g / mol by weight average molecular weight.

[0042] Comparative Example Comparative Example 1 Preparation of Agent A: S1: 200 g of bisphenol A epoxy resin, 150 g of bisphenol F epoxy resin, 350 g of 800 mesh heavy calcium carbonate, 150 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 10 g of thixotropic agent, and 0.1 g of red paste were put into a stirring kettle, and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an agent A intermediate; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight-average molecular weight of 700 g / mol, 350 g of 800 mesh heavy calcium carbonate, 150 g of stearic acid-modified light calcium carbonate obtained in Preparation Example 2, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring tank and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min under vacuum at a stirring speed of 1000 r / min to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0043] Comparative Example 2 Preparation of Agent A: S1: 200g of bisphenol A epoxy resin, 50g of bisphenol F epoxy resin, 350g of 800-mesh heavy calcium carbonate, 150g of 2000-mesh light calcium carbonate, 20g of titanium dioxide, 10g of thixotropic agent, and 0.1g of red paste were added into a stirring kettle, and stirred at a low speed for 10min at a stirring speed of 300r / min, and then stirred at a high speed for 30min at a stirring speed of 1000r / min under vacuum to obtain an agent A intermediate; S2: Add 70g of active diluent and the remaining 150g of bisphenol A epoxy resin into the intermediate product of Agent A, and stir at a low speed of 300r / min for 10min, then stir at a high speed of 1000r / min for 20min under vacuum, and filter, fill and package to obtain Agent A; Preparation of Agent B: S1. 220 g of a polyamide curing agent having an amine value of 200 mg KOH / g and a weight average molecular weight of 700 g / mol, 350 g of 800 mesh heavy calcium carbonate, 150 g of 2000 mesh light calcium carbonate, 20 g of titanium dioxide, 20 g of a thixotropic agent, and 0.1 g of a green slurry were added to a stirring tank and stirred at a low speed for 10 min at a stirring speed of 300 r / min, and then stirred at a high speed for 30 min at a stirring speed of 1000 r / min under vacuum to obtain an intermediate product of Agent B; S2. Add 10 g of curing accelerator, 10 g of silane coupling agent and 220 g of fatty amine curing agent into the intermediate product of Agent B, and stir at low speed for 10 min at a stirring speed of 300 r / min, then stir at high speed for 20 min under vacuum at a stirring speed of 1000 r / min, filter, fill and package to obtain Agent B; 200 g of agent A and 100 g of agent B were mixed evenly to obtain a high-performance epoxy filling repair adhesive.

[0044] Performance test test 1: Referring to the standard ISO4587, the shear strength of the adhesives prepared in each embodiment and comparative example was tested, and the test results are summarized in Table 1: Test 2: The hardness of the adhesives prepared in each embodiment and comparative example was tested according to standard ISO 868. The test results are summarized in Table 1: Table 1 In combination with Examples 1-3, Comparative Examples 1-2 and Table 1, the A and B agents prepared in the present application by using components in a certain mass ratio and preparation steps have higher bonding strength and hardness.

[0045] In combination with Example 1 and Examples 4-7, the present application further improves the bonding strength and hardness of the adhesive by limiting the particle size of light stearic acid and heavy stearic acid to a certain size and respectively modifying the particle size with stearic acid and epoxy silane coupling agent.

[0046] In combination with Example 4 and Examples 8-10, the present application adds two kinds of polyurethane curing agents with different molecular weights and limits the amine value to a certain value, so that the prepared adhesive has higher bonding strength and hardness.

[0047] This specific embodiment of the present application is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, a person skilled in the art may make modifications to the embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A high performance epoxy filled repair adhesive, Features: The invention comprises agent A and agent B, wherein agent A comprises the following raw materials in parts by mass: 30-35 parts of bisphenol A epoxy resin, 5-10 parts of bisphenol F epoxy resin, 30-40 parts of heavy calcium carbonate, 15-20 parts of surface-treated calcium carbonate, 1-3 parts of titanium dioxide, 1-3 parts of thixotropic agent, 0.01 parts of color paste, and 6.5-8.5 parts of active diluent; agent B comprises the following raw materials in parts by mass: 20-24 parts of polyamide curing agent, 30-40 parts of heavy calcium carbonate, 15-20 parts of surface-treated calcium carbonate, 1-3 parts of titanium dioxide, 1-3 parts of thixotropic agent, 0.01-0.02 parts of color paste, 1-3 parts of curing accelerator, 1-2 parts of silane coupling agent, and 20-24 parts of fatty amine curing agent.

2. The high performance epoxy filled repair adhesive according to claim 1, Features: In the agent A and the agent B, the heavy calcium carbonate is epoxysilane-modified heavy calcium carbonate, and the surface-treated calcium carbonate is stearic acid-modified light calcium carbonate.

3. The high performance epoxy filled repair adhesive according to claim 2, Features: In the agent A and the agent B, the mesh number of the heavy calcium carbonate is 800-1000 mesh, and the mesh number of the light calcium carbonate is 2000-2500 mesh.

4. The high performance epoxy filled repair adhesive according to claim 1, Features: The amine value of the polyamide curing agent is 150-220 mg KOH / g.

5. The high performance epoxy filled repair adhesive according to claim 1, Features: The polyamide curing agent includes a polyamide curing agent with a weight average molecular weight of 500-1000 g / mol and a polyamide curing agent with a weight average molecular weight of 7000-9000 g / mol.

6. The high performance epoxy filled repair adhesive according to claim 1, Features: The reactive diluent includes C12-14 alkyl glycidyl ether.

7. The high performance epoxy filled repair adhesive according to claim 1, Features: The curing accelerator includes 2,4,6-tris(dimethylaminomethyl)phenol.

8. The high performance epoxy filled repair adhesive according to claim 1, Features: The silane coupling agent includes 3-glycidyloxypropyltrimethoxysilane.

9. A method for preparing the high performance epoxy filled repair adhesive according to any one of claims 1 to 7, Features: Mix agent A and agent B in a weight ratio of (1.9-2.2):1 to obtain a high-performance epoxy filling repair adhesive.

10. The method for preparing the high performance epoxy filled repair adhesive according to claim 7, Features: The preparation method of the agent A comprises: S1. mixing part of bisphenol A epoxy resin, bisphenol F epoxy resin, heavy calcium carbonate, surface treated calcium carbonate, titanium dioxide, thixotropic agent and color paste, stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 20-40 minutes under a vacuum state; S2. adding active diluent and the remaining bisphenol A epoxy resin, stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 10-30 minutes under a vacuum state to obtain agent A; The preparation method of the B agent includes: S1. mixing a polyamide curing agent, heavy calcium carbonate, surface-treated calcium carbonate, titanium dioxide, a thixotropic agent, and a color paste, and stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 20-40 minutes under a vacuum state; S2. adding a curing accelerator, a silane coupling agent, and a fatty amine curing agent, and stirring at a low speed for 5-15 minutes, and then stirring at a high speed for 10-30 minutes under a vacuum state to obtain the B agent.

Citation Information

Cited By

  • Solvent-resistant heat-resistant epoxy adhesive and preparation method thereof

    CN120924203A