DP steel plate and continuous annealing process thereof

By optimizing the continuous annealing process of DP steel, including the steps of heating, slow cooling, rapid cooling and rolling reduction, the problem of limited elongation of DP steel cold-rolled plates was solved, and a DP steel plate with high strength and good elongation was achieved. Meet the demand for lightweight vehicles.

CN118792584APending Publication Date: 2024-10-18GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410962197.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

The elongation of existing DP steel cold-rolled plates is relatively limited, making it difficult to meet the lightweight needs of automobiles. Moreover, it is difficult to introduce austenite content in the cold-rolling process, which affects the formability and strength of the steel.

Method used

The continuous annealing process is adopted, including two-phase zone heating, slow cooling, rapid cooling, rolling reduction, rapid cooling again, final cooling and smoothing. The heat treatment process of DP steel is optimized by controlling the heating temperature, cooling speed and cooling method. , improve the elongation and strength of the steel plate.

Benefits of technology

It significantly increases the strength and elongation of DP steel plates (50% higher than conventional products on the market), improves the formability of steel, and meets the lightweight needs of automobiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a DP steel cold-rolled sheet and a continuous annealing process thereof, and particularly relates to the technical field of steel processing. The DP steel cold-rolled sheet is composed of, by mass, 0.04%-0.2% of C, 0.4%-1.5% of Si, 1.6%-3.0% of Mn, smaller than or equal to 0.02% of S, smaller than or equal to 0.025% of P, smaller than or equal to 1.5% of Cr, smaller than or equal to 0.5% of Ni, smaller than or equal to 0.05% of Ti, smaller than or equal to 0.1% of V, smaller than or equal to 0.1% of Nb, smaller than or equal to 0.25% of Mo, smaller than or equal to 0.0003% of H and the balance Fe and inevitable impurities. The continuous annealing process of the DP steel cold-rolled sheet comprises the steps of two-phase region heating and heat preservation, slow cooling, rapid cooling, rolling reduction, rapid cooling again, final cooling, leveling and post-treatment. The DP steel plate prepared through the continuous annealing technology can obtain higher strength under the condition of low carbon and manganese content, and meanwhile better weldability and ductility are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of steel processing, and in particular to a DP steel cold-rolled plate and a continuous annealing process thereof. Background Art

[0002] DP steel is composed of two structures: soft ferrite and hard martensite. Therefore, it has the advantages of low yield strength, high tensile strength, high elongation, and high formability. It is very suitable for the forming and processing of high-strength automotive structural parts. It is now widely used in the production of door rings, anti-collision beams, A-pillars and other components.

[0003] At present, in order to meet the lightweight requirements of automobiles, steel companies have developed steel grades such as DP590, DP780, DP980 and even DP1310. As the strength increases, the elongation decreases, which deteriorates the formability. For this reason, people introduce a higher content of austenite into the dual-phase structure of ferrite and martensite through alloying or process optimization to achieve the TRIP effect and thus improve the elongation, forming the so-called DH steel.

[0004] Currently, cold-rolled DP steel is primarily produced using an advanced continuous annealing process, which includes two-phase heating and holding, slow cooling, rapid cooling, overaging, final cooling (air, water, or both), tempering, post-processing, and coiling and packaging. Because this heat treatment process presents significant challenges in introducing austenite, the potential for increasing DP steel's elongation is limited. Summary of the Invention

[0005] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a DP steel cold-rolled sheet, which is composed of the following components in percentage by mass:

[0006] C: 0.04%-0.2%, Si: 0.4%-1.5%, Mn: 1.6%-3.0%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0007] The continuous annealing process of the DP steel plate comprises the following steps:

[0008] (1) Heating: Two-phase zone heating and heat preservation, heat the DP steel cold-rolled sheet to the two-phase zone in a continuous annealing furnace, the heating temperature is 740℃-860℃, and the heat preservation is 4-30 minutes;

[0009] (2) Slow cooling: Slowly cool the heated DP steel plate to 660℃-730℃ at a cooling rate of 1-6℃ / s;

[0010] (3) Rapid cooling: Use air cooling or mist cooling process to quickly cool the temperature of the slow-cooled DP steel plate to 380℃-440℃, with a cooling rate of ≥8℃ / s;

[0011] (4) Rolling reduction: The DP steel plate after rapid cooling is rolled down at 380℃-440℃ with a reduction rate of 5%-40%;

[0012] (5) Rapid cooling again: air-cool the DP steel plate after pressing, and the cooling rate should be ≥

[0013] 8℃ / s, so that the temperature of DP steel plate drops to 220℃-320℃; and keep it in this temperature range for 5-20 minutes;

[0014] (6) Final cooling: Use air cooling, water cooling, water mist cooling or air cooling followed by water cooling to cool the DP steel plate to room temperature after rapid cooling again;

[0015] (7) Leveling: The DP steel plate after final cooling is leveled in a single or double pass, with an elongation of 0.3%-1.2%;

[0016] (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0017] Compared with the prior art, the present invention relates to a DP steel cold-rolled sheet and a continuous annealing process thereof. The DP steel sheet produced by this process has a strength more than 50% higher than conventional products of the same grade on the market and has good elongation. DETAILED DESCRIPTION

[0018] Specific embodiment 1: A DP steel cold-rolled plate is composed of the following components in percentage by mass:

[0019] C: 0.15%, Si: 0.9%, Mn: 2.4%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0020] The continuous annealing process for a DP steel cold-rolled sheet comprises the following steps:

[0021] (1) Heating and holding in two-phase region: the DP steel cold-rolled sheet is heated to the two-phase region in an annealing furnace at a temperature of 800°C and held for 15 minutes;

[0022] (2) Slow cooling: slowly cool the heated DP steel plate to 700°C at a cooling rate of 5°C / s;

[0023] (3) Rapid cooling: The slow-cooled DP steel plate is rapidly cooled by air cooling to a temperature of 410°C at a cooling rate of 20°C / s;

[0024] (4) Rolling reduction: The DP steel plate is rolled down at 400°C with a reduction rate of 20% using a roller; (5) Rapid cooling: The rolled DP steel plate is rapidly cooled again using air cooling at a cooling rate of 15°C / s, so that the temperature of the DP steel plate drops to 250°C; and the plate is aged in this temperature range for 10 minutes;

[0025] (6) Final cooling: the DP steel plate after rapid cooling is first air-cooled to 180°C, and then water-quenched to room temperature;

[0026] (7) Flattening: the final cooled DP steel plate is flattened in a single pass with an elongation of 0.6%;

[0027] (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0028] Specific embodiment 2: A DP steel cold-rolled plate is composed of the following components in percentage by mass:

[0029] C: 0.15%, Si: 0.9%, Mn: 2.4%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0030] The continuous annealing process for a DP steel cold-rolled sheet comprises the following steps:

[0031] (1) Heating and holding in two-phase region: the DP steel cold-rolled sheet is heated to the two-phase region in an annealing furnace at a temperature of 800°C and held for 15 minutes;

[0032] (2) Slow cooling: slowly cool the heated DP steel plate to 680°C at a cooling rate of 5°C / s;

[0033] (3) Rapid cooling: the DP steel plate after slow cooling is rapidly cooled by air cooling, so that the temperature of the DP steel plate is rapidly cooled to 420°C at a cooling rate of 20°C / s;

[0034] (4) Rolling reduction: the rapidly cooled DP steel plate is rolled at 420°C with a reduction rate of 20%;

[0035] (5) Rapid cooling again, air cooling the pressed DP steel plate, cooling rate is 15℃ / s, the temperature of the DP steel plate drops to 230℃; and over-aging at this temperature for 10 minutes;

[0036] (6) Final cooling: the DP steel plate that has been rapidly cooled again is first air-cooled to 180°C and then water-quenched to room temperature;

[0037] (7) Flattening: flatten the DP steel plate in a single pass with an elongation of 0.8%;

[0038] (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0039] Specific embodiment 3: A DP steel cold-rolled plate is composed of the following components in percentage by mass:

[0040] C: 0.15%, Si: 0.9%, Mn: 2.4%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0041] The continuous annealing process for a DP steel cold-rolled sheet comprises the following steps:

[0042] (1) Heating and holding in two-phase region: the DP steel cold-rolled sheet was heated to the two-phase region in an annealing furnace at a temperature of 790°C and held for 15 minutes;

[0043] (2) Slow cooling: slowly cool the heated DP steel plate to 730°C at a cooling rate of 6°C / s;

[0044] (3) Rapid cooling: air-cool the DP steel plate after slow cooling to rapidly cool the temperature of the DP steel plate to 420°C at a cooling rate of 20°C / s;

[0045] (4) Rolling reduction: the DP steel plate after rapid cooling is rolled at 420°C with a reduction rate of 20%;

[0046] (5) Rapid cooling again, air cooling the pressed DP steel plate at a cooling rate of 18°C / s, so that the temperature of the DP steel plate drops to 240°C; and overaging at this temperature for 8 minutes;

[0047] (6) Final cooling: water-cool the DP steel plate after rapid cooling again to room temperature;

[0048] (7) Flattening: flatten the DP steel plate in a single pass with an elongation of 1.0%;

[0049] (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0050] Specific embodiment 4: A DP steel cold-rolled plate, composed of the following components in percentage by mass:

[0051] C: 0.15%, Si: 0.9%, Mn: 2.4%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0052] The continuous annealing process for a DP steel cold-rolled sheet comprises the following steps:

[0053] (1) Heating and holding in two-phase region: heat the DP steel plate in the annealing furnace to the two-phase region at a temperature of 800°C and hold for 15 minutes;

[0054] (2) Slow cooling: slowly cool the heated DP steel plate to 700°C at a cooling rate of 6°C / s;

[0055] (3) Rapid cooling: The DP steel plate is rapidly cooled by air cooling to a temperature of 410°C at a cooling rate of 20°C / s;

[0056] (4) Rolling reduction: the DP steel plate after rapid cooling is rolled down at 400°C with a reduction rate of 20%;

[0057] (5) Rapid cooling again, air cooling the pressed DP steel plate at a cooling rate of 20°C / s, so that the temperature of the DP steel plate drops to 250°C; and overaging at this temperature for 10 minutes;

[0058] (6) Final cooling: cool the DP steel plate that has been rapidly cooled again to 180°C by air cooling, and then water quench the DP steel plate to room temperature;

[0059] (7) Flattening: the DP steel plate after final cooling is flattened in a single pass with an elongation of 0.6%;

[0060] (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0061] Specific embodiment 5: A DP steel cold-rolled plate, composed of the following components in percentage by mass:

[0062] C: 0.04%, Si: 0.4%, Mn: 1.6%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0063] The continuous annealing process for a DP steel cold-rolled sheet comprises the following steps:

[0064] (1) Heating and holding in two-phase region: heat the DP steel plate to the two-phase region in an annealing furnace at a temperature of 800°C and hold for 20 minutes;

[0065] (2) Slow cooling: slowly cool the heated DP steel plate to 680°C at a cooling rate of 5°C / s;

[0066] (3) Rapid cooling: air-cool the slowly cooled DP steel plate to rapidly cool the temperature of the DP steel plate to 420°C at a cooling rate of 20°C / s;

[0067] (4) Rolling reduction: the DP steel plate after rapid cooling is rolled down at 380°C with a reduction rate of 20%; (5) Rapid cooling again: the DP steel plate after rapid cooling is gas-cooled at a cooling rate of 20°C / s, so that the temperature of the DP steel plate is quickly reduced to 230°C; and overaging is performed at this temperature for 10 minutes;

[0068] (6) Final cooling: the DP steel plate that has been rapidly cooled again is cooled to 180°C by air cooling, and then the DP steel plate is water quenched to room temperature;

[0069] (7) Flattening: the DP steel plate after final cooling is flattened in two passes, with an elongation of 0.6%;

[0070] (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0071] Specific embodiment 6: A DP steel cold-rolled plate, composed of the following components in percentage by mass:

[0072] C: 0.2%, Si: 1.5%, Mn: 3.0%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

[0073] The continuous annealing process for a DP steel cold-rolled sheet comprises the following steps:

[0074] (1) Heating and holding in two-phase region: heat the DP steel plate to the two-phase region in an annealing furnace at a temperature of 790°C and hold for 15 minutes;

[0075] (2) Rapid cooling: The heated DP steel is gas cooled to rapidly cool the temperature of the DP steel plate from 790°C to 420°C at a cooling rate of 20°C / s;

[0076] (3) Rolling reduction: the DP steel plate after rapid cooling is rolled at 420°C with a reduction rate of 20%;

[0077] (4) Rapid cooling again, gas cooling the rolled DP steel plate at a cooling rate of 20°C / s, so that the temperature of the DP steel plate drops to 240°C; and overaging at this temperature for 8 minutes;

[0078] (5) Final cooling: air-cool the DP steel plate after rapid cooling again and then water-cool it to room temperature;

[0079] (6) Flattening: the DP steel plate after final cooling is flattened in a single pass with an elongation of 0.6%;

[0080] (7) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

[0081] The following table shows the mechanical properties of DP steel plates produced by conventional processes on the market.

[0082]

[0083] Compared with the mechanical properties of DP steel plates prepared by conventional processes on the market, the following table shows the mechanical properties of DP steel plates prepared by various specific embodiments of the present invention, as shown in the following table:

[0084]

[0085]

[0086] From the comparison of the data in the two tables, it can be seen that the present invention relates to a DP steel plate and a continuous annealing process thereof. The DP steel plate prepared by the process has greatly improved strength and good elongation.

Claims

1. A DP steel plate, characterized in that: It is composed of the following components in percentage by mass: C: 0.04%-0.2%, Si: 0.4%-1.5%, Mn: 1.6%-3.0%, S≤0.02%, P≤0.025%, Cr≤1.5%, Ni≤0.5%, Ti≤0.05%, V≤0.1%, Nb≤0.1%, Mo≤0.25%, H≤0.0003%, and the rest is Fe.

2. A continuous annealing process for DP steel cold-rolled sheet according to claim 1, characterized in that The steps are: (1) Heating: Two-phase zone heating and heat preservation. The DP steel cold-rolled sheet is heated to the two-phase zone in a continuous annealing furnace at a heating temperature of 740°C-860°C and kept warm for 4-30 minutes; (2) Slow cooling: Slowly cool the heated DP steel plate to 660℃-730℃, with a cooling rate of 1-6℃ / s; (3) Rapid cooling: Use air cooling or mist cooling process to quickly cool the temperature of the slow-cooled DP steel plate to 380℃-440℃, with a cooling rate of ≥8℃ / s; (4) Rolling reduction: The DP steel plate after rapid cooling is rolled down at a temperature of 380°C-440°C, with a reduction rate of 5%-40%; (5) Rapid cooling again: air-cool the DP steel plate after pressing, with a cooling rate of ≥8°C / s, so that the temperature of the DP steel plate drops to 220°C-320°C; and keep it in this temperature range for 5-20 minutes; (6) Final cooling: Use air cooling, water cooling, water mist cooling or air cooling followed by water cooling to cool the DP steel plate to room temperature after rapid cooling again; (7) Leveling: The DP steel plate after final cooling is leveled in a single or double pass, with an elongation of 0.3%-1.2%; (8) Post-processing: the flattened DP steel plate is oiled and coiled as required to obtain the DP steel plate of the present invention.

Citation Information

Cited By

  • DP steel for outer covering part and preparation method of DP steel

    CN121951381A