High-strength bubble-free bonding method for silicon carbide seed crystals

By etching the silicon carbide seed crystal bonding surface to form continuous grooves and using potassium hydroxide to etch, the problem of bubble defects in the growth of silicon carbide crystals is solved, high-strength bubble-free bonding and a uniform bonding surface are achieved, and the crystal quality is improved. Growth quality.

CN118792740APending Publication Date: 2024-10-18湖南金博碳基材料研究院有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410826428.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

During the growth process of silicon carbide crystals, the traditional seed crystal bonding method is prone to bubble defects, which affects the bonding strength and crystal growth quality, and the existing ion bombardment method causes uneven distribution of depressions.

Method used

By etching a number of criss-crossing grooves on the bonding surface of the seed crystal, and using potassium hydroxide powder to etch under heating conditions to form etching grooves, continuous etching grooves are formed to enhance the bonding strength and lead out bubbles.

Benefits of technology

It achieves high-strength bubble-free bonding, improves the roughness and adhesion of the bonding surface, while reducing the chance of bubbles, ensuring high-quality crystal growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118792740A_ABST
    Figure CN118792740A_ABST
Patent Text Reader

Abstract

The invention provides a high-strength bubble-free bonding method of a silicon carbide seed crystal, which comprises the following steps: step 1, etching a plurality of crisscrossed etching grooves on the bonding surface of the seed crystal, the etching grooves being through grooves; and step 2, carrying out seed crystal bonding on the bonding surface of the seed crystal. According to the method, the continuous etching grooves are formed through an etching method, so that the bubbles are led out through the etching grooves while firm bonding is guaranteed, and the probability that the bubbles appear in the bonding process is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon carbide, and mainly relates to a high-strength bubble-free bonding method for silicon carbide seed crystals. Background Art

[0002] Silicon carbide (SiC) is a typical wide bandgap semiconductor material and is the third generation semiconductor material after silicon and gallium arsenide. Compared with silicon and gallium arsenide, silicon carbide has excellent properties such as high thermal conductivity, high breakdown field strength, and high saturated electron drift rate. It has great application prospects in high temperature, high frequency, high power and radiation-resistant devices. Since traditional silicon-based power electronic devices have approached the limit of silicon materials that can be achieved due to parasitic effects, the development of semiconductor devices with wide bandgap materials such as SiC has become a development direction.

[0003] In silicon carbide crystal growth technology, the seed crystal bonding process is an important link that affects the quality of later crystal growth. Seed crystal bonding technology generally refers to the technology of bonding the initial seed crystal (sic seed crystal) used for crystal growth with the related components of the single crystal growth system (generally graphite material). Its purpose is to protect the back of the seed crystal, inhibit the volatilization of the back of the seed crystal at high temperature and then ablation, and induce defects such as holes and microtubes during the single crystal growth process.

[0004] The bubbles generated during the seed crystal bonding process are bonding defects. The corresponding position is generally overheated and produces back-end volatilization and ablation. Inducing defects such as holes and microtubes. Therefore, the generation of bubbles must be avoided. At the same time, the industry's SIC crystal growth thickness has further increased, which has put forward higher requirements for bonding strength.

[0005] In this regard, the invention patent CN202310767051 "Silicon Carbide Seed Crystal Bonding Method" proposes a solution to enhance the bonding strength of the seed crystal, that is, to use bias to accelerate the bombardment of charged ions onto the back of the seed crystal, forming depressions thereon, increasing the contact area of ​​the colloid, and the liquid glue will form mechanical connection forces such as hooks, mortises, and rivets after drying and curing, which is equivalent to the high degree of roughness and large surface area of ​​the bonding surface, and the liquid glue has a large adhesion to the bonding surface. In the comparative patent mentioned above, in order to enhance the bonding strength of the seed crystal, ion bombardment is used to produce sufficient depressions (roughness) on the back of the seed crystal to increase adhesion. This method can enhance adhesion, but because the depressions produced by the bombardment are discretely distributed and discontinuous, uniformity may also be a problem. Summary of the invention

[0006] In order to solve the above problems, the present invention discloses a high-strength bubble-free bonding method for silicon carbide seed crystals.

[0007] In order to achieve the above objectives, the present invention is implemented through the following technical solutions:

[0008] A high-strength bubble-free bonding method for silicon carbide seed crystals, characterized in that it comprises the following steps:

[0009] Step 1, etching a plurality of crisscross etched grooves on the bonding surface of the seed crystal 7, wherein the etched grooves are through grooves;

[0010] Step 2: Bonding the seed crystal to the bonding surface of the seed crystal 7.

[0011] As a further improvement, the depth of the etching grooves is 2 to 5 microns, the distance between adjacent etching grooves is 5 to 10 microns; any two etching grooves are parallel or perpendicular to each other.

[0012] As a further improvement, the etching groove is obtained by processing a high-strength bubble-free bonding preprocessing device for a silicon carbide seed crystal, and the high-strength bubble-free bonding preprocessing device for a silicon carbide seed crystal comprises, from top to bottom, a pressing block 1, a mask plate 2, a stage 3 and a heating platform 4; a thermocouple 5 is inserted into the pressing block 1; a plurality of peripheral receiving grooves 6 corresponding to the etching grooves are opened on the bottom surface of the mask plate 2, and the receiving grooves 6 are filled with corrosive substances, and the outer periphery of the mask plate 2 protrudes downward to form a retaining edge 8.

[0013] In a further improvement, the corrosive substance is potassium hydroxide powder.

[0014] As a further improvement, the depth of the receiving groove 6 is 2-4 mm, and the receiving groove 6 is a rectangular groove.

[0015] As a further improvement, the surface flatness of the mask plate 2 is better than 1 micron.

[0016] As a further improvement, the processing steps of the etching groove are as follows:

[0017] 1.1 Place the seed crystal 7 between the mask plate 2 and the stage 3, with the bonding surface of the seed crystal 7 facing the bottom surface of the mask plate 2;

[0018] 1.2 Heat and melt the corrosive material so that the corrosive material etches a groove on the bonding surface of the seed crystal 7.

[0019] Compared with the existing method, the present invention has the following advantages:

[0020] The present invention forms continuous etching grooves by etching, thereby ensuring firm bonding and guiding out bubbles through the etching grooves, thereby reducing the probability of bubbles appearing during the bonding process. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is a schematic diagram of a top view structure of a mask plate of the present invention;

[0022] Figure 2 Schematic diagram of the side structure of the mask plate

[0023] Figure 3 It is a schematic diagram of the structure of the high-strength bubble-free bonding pre-processing device for silicon carbide seed crystals. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.

[0025] (1) Use alkali corrosion resistant materials (including but not limited to nickel metal) to make Figure 1 The mask plate shown. The mask plate has a certain thickness (typical value 5mm), and one side is grooved, and the groove has a certain depth (typical value 2mm). The grooves are evenly distributed on the entire disk surface. As shown in the figure, an orthogonal rectangular groove structure is used in the schematic diagram of this patent, and the groove spacing is 5mm. The two surfaces of the mask plate are finely processed, and the surface flatness is better than 1 micron.

[0026] (2) Fill the groove with potassium hydroxide powder according to the groove depth. And fit the bonding surface of the seed crystal to be used with the mask plate. Since the surface flatness of the seed crystal and the mask plate is relatively high, the two can be closely matched.

[0027] (3) Figure 2 As shown, the matched seed crystal and mask plate are placed on a stage on the heating table. The stage can be made of graphite. The surface of the stage also has good flatness and is in close contact with the non-bonding surface of the seed crystal to ensure uniform heating distribution.

[0028] (4) Place a gravity block or other equipment that can apply pressure on the top of the mask, with a typical weight of 50 kg, to ensure that the mask and seed crystal fit closely under sufficient pressure.

[0029] (5) Set up the heating table and heat it up, and use Figure 2 The temperature of the mask plate is monitored by a thermometer. When the temperature rises to a certain temperature between 450°C and 600°C, the temperature is kept constant and the potassium hydroxide melts.

[0030] (6) Maintain the constant temperature for a certain period of time (typically 30 minutes at 500 degrees). During the constant temperature time, the potassium hydroxide melt flows in the groove of the mask plate and reacts with the closely attached seed crystal bonding surface. The potassium hydroxide melt etches the seed crystal bonding surface, and due to the presence of the mask plate, the etching is selective, and the seed crystal bonding surface obtained by etching will produce an etched groove corresponding to the mask plate. According to the optimization of the etching time, a seed crystal etching pattern with a depth of about 2 to 5 microns is obtained.

[0031] (7) By Figure 1It can be seen that the etching grooves in the etching pattern of the seed crystal back (bonding surface) finally obtained have the characteristics of uniform distribution and connected distribution. The seed crystal treated as above is used for normal bonding process. Due to the presence of the above-mentioned special pattern etching grooves, on the one hand, the roughness of the seed crystal bonding surface (bonding surface) is increased and the bonding strength is enhanced. On the other hand, the volatile gas generated by the adhesive layer during the pressurized curing process can be discharged from the bonding surface along the above-mentioned continuous grooves. Reduce the probability of bubble generation. Achieve the purpose of high-quality bonding.

[0032] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the invention is described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A high-strength bubble-free bonding method for silicon carbide seed crystals, characterized in that: The steps include: Step 1, etching a plurality of crisscross etched grooves on the bonding surface of the seed crystal (7), wherein the etched grooves are through grooves; Step 2: bonding the seed crystal to the bonding surface of the seed crystal (7).

2. The high-strength bubble-free bonding method for silicon carbide seed crystals according to claim 1, characterized in that: The depth of the etching grooves is 2 to 5 microns, and the distance between adjacent etching grooves is 5 to 10 microns; any two etching grooves are parallel or perpendicular to each other.

3. The high-strength bubble-free bonding method for silicon carbide seed crystals according to claim 1, characterized in that: The etching groove is obtained by processing a high-strength bubble-free bonding pre-processing device for a silicon carbide seed crystal, and the high-strength bubble-free bonding pre-processing device for a silicon carbide seed crystal comprises, from top to bottom, a pressing block (1), a mask plate (2), a stage (3) and a heating stage (4); a thermocouple (5) is inserted into the pressing block (1); a plurality of peripheral receiving grooves (6) corresponding to the etching grooves are formed on the bottom surface of the mask plate (2), and the receiving grooves (6) are filled with corrosive substances, and the outer periphery of the mask plate (2) protrudes downward to form a retaining edge (8).

4. The high-strength bubble-free bonding method for silicon carbide seed crystals according to claim 3, characterized in that: The corrosive substance is potassium hydroxide powder.

5. The high-strength bubble-free bonding method for silicon carbide seed crystals according to claim 3, characterized in that: The depth of the receiving groove (6) is 2 to 4 mm, and the receiving groove (6) is a rectangular groove.

6. The high-strength bubble-free bonding method for silicon carbide seed crystals according to claim 3, characterized in that: The surface flatness of the mask plate (2) is better than 1 micron.

7. The high-strength bubble-free bonding method for silicon carbide seed crystals according to claim 3, characterized in that: The processing steps of the etching groove are as follows: 1.1) placing a seed crystal (7) between the mask plate (2) and the stage (3), with the bonding surface of the seed crystal (7) facing the bottom surface of the mask plate (2); 1.2) Heating and melting the corrosive material so that the corrosive material etches an etching groove on the bonding surface of the seed crystal (7).

Citation Information

Cited By

  • Silicon carbide seed crystal bonding piece and bonding method thereof

    CN120158810A