Modified aramid fiber as well as preparation method and application thereof

By uniformly growing nano-zinc oxide particles on the surface of aramid fiber, the problem of insufficient puncture resistance and interlayer adhesion of existing aramid-epoxy resin composite fabrics is solved, and high-performance composite material preparation is achieved to meet higher standards. application requirements.

CN118792876APending Publication Date: 2024-10-18CIXI HIGH NEW COXIN SEALING MATERIAL
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410837412.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Due to the high content of epoxy resin in existing aramid-epoxy resin composite fabrics, the aramid fiber content is reduced, and the puncture-proof performance and inter-layer adhesion are insufficient, making it difficult to meet the needs of high-demand applications.

Method used

By uniformly growing nano-zinc oxide particles on the surface of the aramid fiber and using double nano-zinc oxide modification treatment, the tensile strength, elongation at break and breaking strength of the fiber are increased, and the structural interlocking between fibers is enhanced to improve the relationship with the environment. Oxygen resin compatibility and bonding effectiveness.

Benefits of technology

It significantly improves the puncture-proof effect and inter-layer adhesion of aramid-epoxy resin composite cloth, reduces the amount of epoxy resin, meets higher standard application requirements, and improves the overall performance of the composite material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004913556460000091
    Figure BDA0004913556460000091
  • Figure BDA0004913556460000101
    Figure BDA0004913556460000101
Patent Text Reader

Abstract

The invention relates to the technical field of aramid fiber modification, in particular to modified aramid fiber and a preparation method and application thereof. According to the preparation method of the modified aramid fiber, the aramid fiber is pretreated, secondary nano-zinc oxide modification is performed, and nano-zinc oxide particles uniformly grow on the surface of the aramid fiber, so that structural interlocking among the aramid fiber is increased, and the roughness of the surface of the fiber is remarkably improved; the prepared modified aramid fiber can significantly improve the tensile strength, elongation at break and breaking strength of the aramid fiber, and further improve the puncture-proof effect and interlayer bonding force of the aramid fiber epoxy resin composite cloth. The modified aramid fiber and epoxy resin composite cloth is prepared from the modified aramid fiber and epoxy resin, on one hand, the use amount of epoxy resin can be reduced, and on the other hand, the problems of layering and poor puncture-proof effect frequently occurring in common aramid fiber and epoxy resin composite cloth are solved. According to the method provided by the invention, the performance of the material is successfully improved by effectively modifying the aramid fiber, so that the material has wider application prospects and economic benefits in the field of composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aramid modification, and in particular to a modified aramid and a preparation method and application thereof. Background Art

[0002] As people's requirements for quality of life continue to increase, they also pay more attention to their own safety and health. Ordinary textiles can no longer meet people's diverse needs, which puts higher requirements on the safety and protective performance of textiles. Therefore, the application areas of fabrics with protective functions are increasing.

[0003] Aramid fiber is a synthetic fiber made from a type of linear polyamide containing aromatic rings. Aramid fiber has excellent properties such as high specific modulus, high specific strength, low density, fatigue resistance, and high temperature resistance. Therefore, it is widely used in aerospace and other fields.

[0004] Due to the high crystallinity of aramid fiber and the lack of active groups on the surface, the bonding between aramid fiber and epoxy resin interface is poor, so a large amount of epoxy resin is required to penetrate to have sufficient bonding strength. Therefore, the mass fraction of epoxy resin in the aramid epoxy resin composite cloth currently on the market is usually as high as 35%-45%. However, when the content of epoxy resin increases and the content of aramid fiber decreases, the protective ability of the stab-proof clothing will be greatly reduced; in addition, relevant studies have shown that even under the above-mentioned high content of epoxy resin, the stab-proof clothing still has the problems of fiber cloth delamination and poor anti-stab effect, which is difficult to meet the use requirements of stab-proof clothing. Summary of the invention

[0005] The purpose of this application is to provide a modified aramid and its preparation method and application in view of the shortcomings of current technology. The modified aramid provided by this application and epoxy resin are used to prepare a modified aramid epoxy resin composite cloth. On the one hand, the amount of epoxy resin used can be reduced, and on the other hand, the problems of delamination and poor anti-stab effect that often occur in ordinary aramid epoxy resin composite cloths are solved. By uniformly growing nano zinc oxide particles on the surface of aramid fibers, the structural interlocking between aramid fibers is increased, and the roughness of the fiber surface is significantly improved. The prepared modified aramid can significantly improve the tensile strength, elongation at break, and breaking strength of aramid fibers, thereby improving the anti-stab effect and interlayer bonding of the aramid epoxy resin composite cloth.

[0006] In a first aspect, the present application provides a method for preparing modified aramid fiber, which adopts the following technical scheme: A method for preparing modified aramid fiber comprises the following steps: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 20-30 minutes, wash it with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 20-30 minutes, and wash it with deionized water to remove impurities on the surface of the aramid fiber; S2, mixing the zinc acetate solution and the sodium hydroxide solution to obtain a mixed solution, then heating to 60° C. and keeping the temperature for 1-2 hours, immersing the aramid fiber treated in step S1 in the mixed solution, and performing a first reaction under ultrasonic stirring, drying the aramid fiber after the first reaction to obtain a first nano zinc oxide modified aramid fiber; S3. Mix the zinc nitrate solution and the urotropine solution to obtain a mixed solution of zinc nitrate and urotropine, then heat it to 60°C and keep it warm for 1 hour, immerse the first nano zinc oxide modified aramid fiber in the mixed solution of zinc nitrate and urotropine, and carry out a second reaction under ultrasonic stirring. Dry the aramid fiber after the second reaction at a temperature of 145°C for 2-3 hours to obtain modified aramid.

[0007] By adopting the above technical scheme, step S1: pre-treating aramid fiber, in this step, the aramid fiber is first immersed in a sodium hydroxide solution and then washed with deionized water. In this process, the sodium hydroxide solution can remove grease and other impurities on the surface of the aramid fiber and improve the purity of the fiber. Then, the aramid fiber is immersed in an acetic acid solution, which can further clean the fiber surface and provide a good foundation for the subsequent growth of nano zinc oxide. Step S2: the first nano zinc oxide modification, in this step, a solution formed by mixing zinc acetate and sodium hydroxide is used to grow nano zinc oxide particles on the surface of the aramid fiber. This process is carried out under ultrasonic stirring to ensure that the zinc oxide particles are evenly distributed on the fiber surface. This modification can improve the mechanical properties of the aramid fiber, such as tensile strength and elongation at break, while also enhancing the structural interlocking between the fibers and improving the interlayer bonding of the composite material. Step S3: the second nano zinc oxide modification, this step uses a mixed solution of zinc nitrate and urotropine to further modify the aramid fiber. This process is also carried out under ultrasonic stirring to ensure a more uniform distribution of nano zinc oxide particles. The second modification can further improve the mechanical properties and interlayer bonding of the fiber. These three steps work together to make the surface of the aramid fiber rougher, increase the contact area and friction between the fibers, and thus improve the structural interlocking effect. This helps to improve the stab-proof effect and interlayer bonding of the aramid epoxy resin composite cloth. Through this double nano-zinc oxide modification, the tensile strength, elongation at break and breaking strength of the aramid fiber are significantly improved, and these improved mechanical properties are directly reflected in the performance of the final composite material. In summary, the modified aramid preparation method provided in the present application effectively improves the mechanical properties of the aramid fiber through two-stage nano-zinc oxide modification, while improving the compatibility and bonding effect with epoxy resin, thereby preparing a composite cloth material with excellent stab-proof performance and high bonding strength.

[0008] Preferably, in step S2, the molar concentration of the zinc acetate solution is 0.2-0.25 mol / L, the molar concentration of the sodium hydroxide solution is 0.25-0.28 mol / L, and the volume ratio of the zinc acetate solution to the sodium hydroxide solution is 1:1-1.2.

[0009] By adopting the above technical scheme, in step S2, the specific molar concentration and volume ratio of zinc acetate solution and sodium hydroxide solution have specific functions and synergistic effects in the present application. The molar concentration of zinc acetate solution is 0.2-0.25 mol / L, while the molar concentration of sodium hydroxide solution is 0.25-0.28 mol / L, and the volume ratio of the two solutions is maintained at 1:1-1.2 when mixed. Such concentration and ratio configuration are crucial for preparing modified aramid fibers, and the specific effects are as follows: the appropriate molar concentration helps to maintain the uniform distribution of reactants during the mixing process, so that nano zinc oxide particles can grow more evenly on the surface of the aramid fibers. This uniformity is a key factor in improving the performance of the final product. By accurately controlling the molar concentrations of zinc acetate and sodium hydroxide, the rate of formation of nano zinc oxide in the mixed solution can be adjusted. Too fast or too slow a reaction rate may lead to an undesirable fiber surface modification effect. The uniform growth of nano zinc oxide increases the structural interlocking between aramid fibers, which improves the interlayer bonding and stab-proof effect of the composite cloth. Appropriate molar concentration and volume ratio are conducive to forming an ideal zinc oxide particle size and distribution, thereby enhancing the structural interlocking effect. In general, the specific molar concentration and volume ratio of zinc acetate and sodium hydroxide in step S2 are designed to achieve precise control of the surface modification process of aramid fibers, thereby solving the problems of delamination and poor stab-proof effect of ordinary aramid epoxy resin composite fabrics without sacrificing the amount of epoxy resin. Through this modification technology, the performance of the composite fabric can be significantly improved to meet higher standards of application requirements.

[0010] Preferably, in step S2, the process conditions of the first reaction are: reaction temperature is 70-75°C, and reaction time is 1-1.5h.

[0011] By adopting the above technical scheme, in step S2, the process conditions of the first reaction are set to specific temperature (70-75°C) and time (1-1.5 hours), which have a significant effect on the effect of preparing modified aramid fiber. The appropriate reaction temperature is conducive to the uniformity and consistency of the reaction of zinc acetate and sodium hydroxide to generate nano zinc oxide particles. Too high or too low temperature may affect the reaction rate and the quality of the product. In the temperature range of 70-75°C, the rate of chemical reaction will be accelerated, which helps to obtain the desired nano zinc oxide growth effect in a short time while avoiding unnecessary energy consumption. The appropriate reaction time ensures that enough nano zinc oxide particles can be formed on the surface of the aramid fiber, increases structural interlocking, improves the surface roughness of the fiber, and thus improves the bonding force with the epoxy resin. Controlling the reaction time and temperature can prevent damage to the aramid fiber caused by excessive reaction and maintain its original mechanical strength and flexibility. In summary, the process conditions in step S2 are carefully designed to ensure the best surface modification effect without damaging the raw materials and create a good foundation for the second nano zinc oxide modification. Such process settings are crucial to the entire modification process and the performance of the final product.

[0012] Preferably, in step S2, the drying process conditions are: drying at a temperature of 120-130° C. for 1.5-2 h.

[0013] Preferably, in step S3, the molar concentration of the zinc nitrate solution is 0.3-0.33 mol / L, the molar concentration of the urotropine solution is 0.15-0.18 mol / L, and the volume ratio of the zinc nitrate solution to the urotropine solution is 1:1.

[0014] By adopting the above technical scheme, the molar concentration of the zinc nitrate solution is 0.3-0.33 mol / L, and the molar concentration of the urotropine solution is 0.15-0.18 mol / L. Such a concentration range helps to ensure that the second nano zinc oxide growth process is carried out uniformly. Uniform reaction is the key to forming nanoparticles of uniform size and distribution, which is crucial for improving the mechanical properties and anti-stab effect of the final product. By adjusting the molar concentration of the reactants, the growth rate and morphology of nano zinc oxide can be controlled. Appropriate molar concentration and volume ratio are conducive to the formation of ideal nano zinc oxide particle size and shape, thereby enhancing the structural interlocking effect and improving the surface roughness of the fiber. The purpose of the second nano zinc oxide modification is to further increase the structural interlocking between aramid fibers and improve the interlayer bonding and anti-stab effect of the composite cloth. Appropriate molar concentration and volume ratio help to form more uniform and dense nano zinc oxide particles, thereby enhancing the structural interlocking effect. The second nano zinc oxide modification further improves the mechanical properties of aramid fibers, including tensile strength, elongation at break and breaking strength. These performance improvements translate into improved overall performance of the composite fabric, especially in terms of stab-proof effect and interlayer adhesion. In general, the design of the molar concentration and volume ratio in step S3 is to achieve precise control of the second modification process of the aramid fiber surface, thereby solving the problems of delamination and poor stab-proof effect of ordinary aramid epoxy resin composite fabrics without sacrificing the amount of epoxy resin. Through this modification technology, the performance of the composite fabric can be significantly improved to meet higher standards of application requirements.

[0015] Preferably, in step S3, the process conditions of the second reaction are: reaction temperature is 80-82° C., and reaction time is 2-2.5 h.

[0016] By adopting the above technical scheme, the appropriate reaction temperature is conducive to the uniformity and consistency of the reaction of zinc nitrate and urotropine to generate nano zinc oxide particles. Too high or too low temperature may affect the reaction rate and the quality of the product. In the temperature range of 80-82°C, the rate of the chemical reaction will be accelerated, which helps to obtain the desired nano zinc oxide growth effect in a short time while avoiding unnecessary energy consumption. The appropriate reaction time ensures that sufficient nano zinc oxide particles can be formed on the surface of the aramid fiber, increases the structural interlocking, improves the surface roughness of the fiber, and thus improves the bonding with the epoxy resin. Controlling the reaction time and temperature can prevent damage to the aramid fiber caused by excessive reaction and maintain its original mechanical strength and flexibility. Through the optimization of the second reaction, the modified aramid fiber obtained shows better compatibility when compounded with epoxy resin, improves the stab-proof effect and interlayer bonding of the composite cloth, and allows the use of epoxy resin to be reduced.

[0017] In a second aspect, the present application provides a modified aramid fiber, which adopts the following technical solution: As a general technical concept, the present application also provides modified aramid fiber prepared by the above-mentioned method for preparing modified aramid fiber.

[0018] In a third aspect, the present application provides an application of modified aramid fiber, using the following technical solution: As a general technical concept, the present application also provides the application of the above-mentioned modified aramid in stab-proof clothing, firstly, the modified aramid is woven into a modified aramid spun plain fabric with a linear density of 333tex, and then a curing agent polyetheramine D230 with a mass ratio of 2:1 is added to the E44 epoxy resin, and stirred evenly to obtain an E44 epoxy resin mixed liquid; the modified aramid spun plain fabric and the E44 epoxy resin mixed liquid are prepared into a modified aramid epoxy resin composite cloth on a flat vulcanizer, and finally the modified aramid epoxy resin composite cloth is made into a stab-proof clothing; modified aramid epoxy resin composite cloths of different thicknesses are prepared by arranging the modified aramid spun plain fabric and the E44 epoxy resin in different layers, wherein the mass content of the modified aramid spun plain fabric in the modified aramid epoxy resin composite cloth is 70%-75%.

[0019] By adopting the above technical solution, by weaving the modified aramid into a plain fabric with a linear density of 333tex, it can be ensured that the fabric has sufficient strength and toughness. Nano zinc oxide particles grow evenly on the fiber surface, increase the structural interlocking between the fibers, improve the overall strength of the fabric, and effectively improve the puncture resistance of the stab-proof clothing. The epoxy resin mixture prepared by mixing E44 epoxy resin with curing agent polyetheramine D230 can be well combined with the modified aramid spun plain fabric. Due to the increase in the roughness of the modified aramid surface, it helps to increase the contact area and adhesion between the resin and the fiber, thereby enhancing the interlayer bonding force of the composite cloth. By combining different layers of modified aramid spun plain fabric with E44 epoxy resin mixture, composite cloths of different thicknesses can be prepared to meet the customization of different protection needs. At the same time, since the tensile strength, elongation at break and breaking strength of the modified aramid fiber are significantly improved, the resulting composite cloth also exhibits better mechanical properties. By using modified aramid, dependence on epoxy resin can be reduced, material costs can be reduced, and environmental impact can be reduced. The mass content of E44 epoxy resin is controlled within the range of 25%-30%, which not only ensures the performance of the composite cloth, but also avoids the use of excessive resin. Due to the excellent performance of the modified aramid fiber, the composite cloth not only has better protective performance, but also improves the comfort when wearing. In addition, the composite cloth also has good durability and can withstand long-term use without being easily damaged. In summary, the application of modified aramid in this application in stab-proof clothing, through the combination with E44 epoxy resin, forms a high-performance composite cloth, which significantly improves the protective ability of the stab-proof clothing while maintaining good cost-effectiveness and environmental protection characteristics.

[0020] In summary, the beneficial technical effects of this application are: 1. Uniform growth of nano zinc oxide particles: By immersing the aramid fiber in a specific solution and performing multiple reaction treatments, nano zinc oxide particles can be uniformly grown on the surface of the aramid fiber. This helps to increase the structural interlocking between the fibers and improves the roughness of the fiber surface.

[0021] 2. Improve fiber performance: The modified aramid fiber shows better tensile strength, elongation at break and breaking strength. This means that the modified aramid is more wear-resistant and durable during use.

[0022] 3. Improved puncture resistance: By uniformly growing nano zinc oxide particles on the surface of aramid fibers, the structural interlocking between fibers is increased, thereby significantly improving the puncture resistance of the composite fabric. This structural interlocking effect enhances the interface strength between the fiber and the resin, allowing the composite fabric to more effectively disperse and absorb energy when subjected to external force impact.

[0023] 4. Improved interlayer adhesion: The increased roughness of the surface of the modified aramid fiber increases the contact area with the epoxy resin, thereby enhancing the interlayer adhesion. This helps prevent the composite fabric from delamination and improves the overall stability and durability of the composite fabric.

[0024] 5. Improved mechanical properties: The tensile strength, elongation at break and breaking strength of the modified aramid fiber are significantly improved. These enhanced mechanical properties are directly converted into high performance of the composite fabric, enabling it to exhibit better toughness and strength when subjected to external forces.

[0025] 6. Reduce material usage: The introduction of modified aramid can reduce the amount of epoxy resin used to a certain extent, thereby saving costs and achieving the purpose of lightweight design. DETAILED DESCRIPTION

[0026] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0027] Example 1 A method for preparing modified aramid fiber comprises the following steps: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 20 minutes, wash it with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 20 minutes, and wash it with deionized water to remove impurities on the surface of the aramid fiber; S2, mixing a zinc acetate solution with a molar concentration of 0.2 mol / L and a sodium hydroxide solution with a molar concentration of 0.25 mol / L in a volume ratio of 1:1 to obtain a mixed solution, then heating to 60°C and keeping warm for 1 hour, immersing the aramid fiber treated in step S1 in the mixed solution, and performing a first reaction under ultrasonic stirring, wherein the process conditions of the first reaction are: a reaction temperature of 70°C, a reaction time of 1.5 hours, and drying the aramid fiber after the first reaction at a temperature of 120°C for 2 hours to obtain a first nano zinc oxide modified aramid fiber; S3. A zinc nitrate solution with a molar concentration of 0.3 mol / L and a urotropine solution with a molar concentration of 0.15 mol / L are mixed in a volume ratio of 1:1 to obtain a mixed solution of zinc nitrate and urotropine, and then the temperature is raised to 60° C. and kept warm for 1 hour, and the first nano zinc oxide modified aramid fiber is immersed in the mixed solution of zinc nitrate and urotropine, and a second reaction is carried out under ultrasonic stirring. The process conditions of the second reaction are: the reaction temperature is 80° C., and the reaction time is 2.5 hours. The aramid fiber after the second reaction is dried at a temperature of 145° C. for 2 hours to obtain modified aramid.

[0028] Example 2 A method for preparing modified aramid fiber comprises the following steps: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 30 minutes, wash it with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 30 minutes, and wash it with deionized water to remove impurities on the surface of the aramid fiber; S2, mixing a zinc acetate solution with a molar concentration of 0.25 mol / L and a sodium hydroxide solution with a molar concentration of 0.28 mol / L in a volume ratio of 1:1.2 to obtain a mixed solution, then heating to 60°C and keeping warm for 2 hours, immersing the aramid fiber treated in step S1 in the mixed solution, and performing a first reaction under ultrasonic stirring, wherein the process conditions of the first reaction are: a reaction temperature of 75°C, a reaction time of 1.5 hours, and drying the aramid fiber after the first reaction at a temperature of 130°C for 1.5 hours to obtain a first nano zinc oxide modified aramid fiber; S3. A zinc nitrate solution with a molar concentration of 0.33 mol / L and a urotropine solution with a molar concentration of 0.18 mol / L are mixed in a volume ratio of 1:1 to obtain a mixed solution of zinc nitrate and urotropine, and then the temperature is raised to 60° C. and kept warm for 1 hour, and the first nano zinc oxide modified aramid fiber is immersed in the mixed solution of zinc nitrate and urotropine, and a second reaction is carried out under ultrasonic stirring. The process conditions of the second reaction are: the reaction temperature is 82° C., and the reaction time is 2 hours. The aramid fiber after the second reaction is dried at a temperature of 145° C. for 3 hours to obtain modified aramid.

[0029] Example 3 A method for preparing modified aramid fiber comprises the following steps: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 25 minutes, wash it with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 25 minutes, and wash it with deionized water to remove impurities on the surface of the aramid fiber; S2, mixing a zinc acetate solution with a molar concentration of 0.23 mol / L and a sodium hydroxide solution with a molar concentration of 0.27 mol / L in a volume ratio of 1:1.1 to obtain a mixed solution, then heating to 60°C and keeping warm for 1.5 hours, immersing the aramid fiber treated in step S1 in the mixed solution, and performing a first reaction under ultrasonic stirring, wherein the process conditions of the first reaction are: a reaction temperature of 73°C, a reaction time of 1.3 hours, and drying the aramid fiber after the first reaction at a temperature of 125°C for 1.8 hours to obtain a first nano zinc oxide modified aramid fiber; S3. A zinc nitrate solution with a molar concentration of 0.32 mol / L and a urotropine solution with a molar concentration of 0.17 mol / L are mixed in a volume ratio of 1:1 to obtain a mixed solution of zinc nitrate and urotropine, and then the temperature is raised to 60° C. and kept warm for 1 hour, and the first nano zinc oxide modified aramid fiber is immersed in the mixed solution of zinc nitrate and urotropine, and a second reaction is carried out under ultrasonic stirring. The process conditions of the second reaction are: the reaction temperature is 81° C., and the reaction time is 2.3 hours. The aramid fiber after the second reaction is dried at a temperature of 145° C. for 2.5 hours to obtain modified aramid.

[0030] Comparative Example 1 A method for preparing modified aramid fiber comprises the following steps: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 25 minutes, wash it with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 25 minutes, and wash it with deionized water to remove impurities on the surface of the aramid fiber; S2. A zinc acetate solution with a molar concentration of 0.23 mol / L and a sodium hydroxide solution with a molar concentration of 0.27 mol / L are mixed in a volume ratio of 1:1.1 to obtain a mixed solution, and then the temperature is raised to 60°C and kept warm for 1.5 hours. The aramid fiber treated in step S1 is immersed in the mixed solution and reacted under ultrasonic stirring. The process conditions of the reaction are: reaction temperature of 73°C, reaction time of 3.6 hours, and the reacted aramid fiber is dried at a temperature of 145°C for 2.5 hours to obtain modified aramid fiber.

[0031] Comparative Example 2 A method for preparing modified aramid fiber comprises the following steps: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 25 minutes, wash it with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 25 minutes, and wash it with deionized water to remove impurities on the surface of the aramid fiber; S2. A zinc nitrate solution with a molar concentration of 0.32 mol / L and a urotropine solution with a molar concentration of 0.17 mol / L are mixed in a volume ratio of 1:1 to obtain a mixed solution of zinc nitrate and urotropine, and then the temperature is raised to 60° C. and kept warm for 1 hour. The aramid fiber treated in step S1 is immersed in the mixed solution of zinc nitrate and urotropine, and reacted under ultrasonic stirring. The process conditions of the reaction are: reaction temperature of 81° C., reaction time of 3.6 hours. The aramid fiber after the reaction is dried at a temperature of 145° C. for 2.5 hours to obtain modified aramid.

[0032] Performance Testing The modified aramid fibers and aramid fibers prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were sampled and subjected to the following performance tests. The test results are shown in Table 1. Tensile strength and elongation at break: measured in accordance with the provisions of GB / T14337-2008; Breaking strength: measured in accordance with the provisions of DB51 / T1916.6-2014; Table 1 Performance test project Tensile strength / GPa Elongation at break / % Breaking strength / cN / dtex Example 1 3.21 7.3 21.7 Example 2 3.45 7.1 22.6 Example 3 3.32 7.4 22.3 Comparative Example 1 2.85 6.8 19.7 Comparative Example 2 3.06 6.9 20.4 Aramid fiber 2.56 6.3 17.8 Analyzing the data in Table 1, we can see that: 1) The modified aramid prepared in Example 1 to Example 3 has excellent tensile strength, elongation at break and breaking strength, indicating that the present application uniformly grows nano zinc oxide particles on the surface of aramid fibers, increases the structural interlocking between aramid fibers, and significantly improves the roughness of the fiber surface. The prepared modified aramid can significantly improve the tensile strength, elongation at break and breaking strength of the aramid fibers, thereby improving the puncture-proof effect and interlayer bonding strength of the aramid epoxy resin composite cloth.

[0033] 2) The comparative analysis of the performance of the modified aramid fibers obtained in Example 3 and Comparative Examples 1-2 shows that the secondary nano zinc oxide modification of the present application further improves the mechanical properties of the aramid fibers, including tensile strength, elongation at break and breaking strength. These performance improvements translate into improved overall performance of the composite fabric, especially in terms of stab-proof effect and interlayer adhesion.

[0034] Application Example 1: Stab-proof clothing The modified aramid prepared in Example 3 is first woven into a modified aramid spun plain fabric with a linear density of 333 tex, and then 2 kg of E44 epoxy resin and 1 kg of curing agent polyetheramine D230 are fully mixed and vacuumed for 40 minutes to remove bubbles to obtain an E44 epoxy resin mixed solution; the modified aramid spun plain fabric and the E44 epoxy resin mixed solution are made into a modified aramid epoxy resin composite cloth on a flat vulcanizer to prepare a layer of modified aramid spun plain fabric and a layer of E44 epoxy resin modified aramid epoxy resin composite cloth, wherein the mass content of the modified aramid spun plain fabric in the modified aramid epoxy resin composite cloth is 73%, and finally the modified aramid epoxy resin composite cloth is made into a stab-proof clothing.

[0035] Application Example 2: Stab-proof clothing The modified aramid prepared in Example 3 is first woven into a modified aramid spun plain fabric with a linear density of 333 tex, and then 2 kg of E44 epoxy resin and 1 kg of curing agent polyetheramine D230 are fully mixed and vacuumed for 40 minutes to remove bubbles to obtain an E44 epoxy resin mixed solution; the modified aramid spun plain fabric and the E44 epoxy resin mixed solution are made into a modified aramid epoxy resin composite cloth on a flat vulcanizer to prepare 2 layers of modified aramid spun plain fabric and 1 layer of E44 epoxy resin modified aramid epoxy resin composite cloth, wherein the mass content of the modified aramid spun plain fabric in the modified aramid epoxy resin composite cloth is 73%; finally, the modified aramid epoxy resin composite cloth is made into a stab-proof clothing.

[0036] Application Example 3: Stab-proof clothing The modified aramid prepared in Example 3 is first woven into a modified aramid spun plain fabric with a linear density of 333 tex, and then 2 kg of E44 epoxy resin and 1 kg of curing agent polyetheramine D230 are fully mixed and vacuumed for 40 minutes to remove bubbles to obtain an E44 epoxy resin mixed solution; the modified aramid spun plain fabric and the E44 epoxy resin mixed solution are made into a modified aramid epoxy resin composite cloth on a flat vulcanizer to prepare 2 layers of modified aramid spun plain fabric and 2 layers of modified aramid epoxy resin composite cloth of E44 epoxy resin, wherein the mass content of the modified aramid spun plain fabric in the modified aramid epoxy resin composite cloth is 73%, and finally the modified aramid epoxy resin composite cloth is made into a stab-proof clothing.

[0037] Application Comparative Example 1 Stab-proof Clothing The same as the comparative example 1, except that the modified aramid is the modified aramid prepared in the comparative example 1.

[0038] Application Comparative Example 2 Stab-Proof Clothing The same as the comparative example 1, except that the modified aramid is the modified aramid prepared in the comparative example 2.

[0039] Application Comparative Example 3 Stab-Proof Clothing The same as the comparative example 1, except that aramid is used instead of modified aramid.

[0040] Application performance testing The stab-resistant clothing prepared in Application Example 1, Application Example 3 and Application Comparative Example 1 to Application Comparative Example 3 were sampled and subjected to the following performance tests. The test results are shown in Table 2. Stab-proof effect: According to GA68-2019 "Police Stab-proof Clothing", the puncture tester is used for measurement; Interlaminar shear strength: measured in accordance with the provisions of GB1461-1988.

[0041] Table 2 Application performance test Note: “—” in Table 2 means no test was performed.

[0042] Analyzing the data in Table 2, we can see that: 1) The stab-proof clothing prepared in Application Examples 1 to 3 has excellent stab-proof effect and interlayer adhesion. At the same time, the test results show that as the number of modified aramid plain weave fabric E44 epoxy resin layers increases, its combined buffering effect is better and the puncture-proof effect is more significant.

[0043] 2) The performance comparison analysis of the stab-resistant clothing prepared in combination with Application Example 1 and Application Comparative Example 1-Application Comparative Example 2 shows that the secondary nano zinc oxide modification of the present application further improves the mechanical properties of the aramid fiber, including tensile strength, elongation at break and breaking strength. These performance improvements translate into improved overall performance of the composite fabric, especially in terms of stab-resistant effect and interlayer bonding.

[0044] 3) The comparative analysis of the performance of the stab-resistant clothing prepared in combination with Application Example 1 and Comparative Example 3 shows that the modified aramid prepared in the present application and the epoxy resin are used to prepare the modified aramid epoxy resin composite cloth, which can reduce the amount of epoxy resin used in the stab-resistant clothing on the one hand, and solve the problems of delamination and poor stab-resistant effect often seen in ordinary aramid epoxy resin composite cloths on the other hand.

[0045] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A method for preparing modified aramid fiber, characterized in that: The following steps are involved: S1. Immerse the aramid fiber in a 10% sodium hydroxide solution for 20-30 minutes, wash with deionized water, and then immerse the washed aramid fiber in a 30% acetic acid solution for 20-30 minutes, and wash with deionized water to remove impurities on the surface of the aramid fiber; S2, mixing the zinc acetate solution and the sodium hydroxide solution to obtain a mixed solution, then heating to 60° C. and keeping the temperature for 1-2 hours, immersing the aramid fiber treated in step S1 in the mixed solution, and performing a first reaction under ultrasonic stirring, drying the aramid fiber after the first reaction to obtain a first nano zinc oxide modified aramid fiber; S3. Mix the zinc nitrate solution and the urotropine solution to obtain a mixed solution of zinc nitrate and urotropine, then heat it to 60°C and keep it warm for 1 hour, immerse the first nano zinc oxide modified aramid fiber in the mixed solution of zinc nitrate and urotropine, and carry out a second reaction under ultrasonic stirring. Dry the aramid fiber after the second reaction at a temperature of 145°C for 2-3 hours to obtain modified aramid.

2. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S2, the molar concentration of the zinc acetate solution is 0.2-0.25 mol / L, and the molar concentration of the sodium hydroxide solution is 0.25-0.28 mol / L.

3. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S2, the volume ratio of the zinc acetate solution to the sodium hydroxide solution is 1:1-1.

2.

4. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S2, the process conditions of the first reaction are: reaction temperature is 70-75°C, and reaction time is 1-1.5h.

5. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S2, the drying process conditions are: drying at a temperature of 120-130°C for 1.5-2h.

6. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S3, the molar concentration of the zinc nitrate solution is 0.3-0.33 mol / L, and the molar concentration of the hexamethylenetetramine solution is 0.15-0.18 mol / L.

7. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S3, the volume ratio of the zinc nitrate solution to the hexamine solution is 1:

1.

8. The method for preparing modified aramid fiber according to claim 1, characterized in that: In step S3, the process conditions of the second reaction are: reaction temperature is 80-82°C, and reaction time is 2-2.5h.

9. A modified aramid fiber, characterized in that: The modified aramid fiber is prepared by the preparation method of any one of claims 1 to 8.

10. The use of the modified aramid fiber in stab-proof clothing according to claim 9, characterized in that: First, the modified aramid is spun into a modified aramid plain fabric with a linear density of 333tex, and then a curing agent polyetheramine is added to E44 epoxy resin in a mass ratio of 2:1, and the mixture is stirred evenly to obtain an E44 epoxy resin mixed solution; the modified aramid plain fabric and the E44 epoxy resin mixed solution are prepared into a modified aramid epoxy resin composite cloth on a flat vulcanizer, and finally the modified aramid epoxy resin composite cloth is made into a stab-proof clothing; modified aramid epoxy resin composite cloths of different thicknesses are prepared by arranging the modified aramid plain fabric and the E44 epoxy resin in different numbers of layers, wherein the mass content of the modified aramid plain fabric in the modified aramid epoxy resin composite cloth is 70%-75%.

Citation Information

Cited By

  • High-strength modified aramid nanofiber as well as preparation method and application thereof

    CN120867095A

  • High-strength modified aramid nanofiber, and preparation method and application thereof

    CN120867095B

  • High-strength and high-modulus polyethylene composite yarn as well as preparation method and application thereof

    CN121321407A