Moisture-absorbing breathable fabric and preparation method thereof
Through the biological enzyme washing treatment and treatment liquid immersion technology of polyester fiber and carbon fiber blends and modified polyamide fiber, the problem of insufficient breathability and moisture absorption performance of the fabric has been solved, and the coordinated improvement of moisture absorption, breathability and mechanical properties of the fabric has been achieved, and Improves the acid and alkali resistance stability of the fabric.
Patent Information
- Application Number
- CN202410753332.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing fabrics have deficiencies in breathability and moisture absorption properties, and their mechanical properties are prone to deterioration. It is difficult to achieve coordinated improvements in moisture absorption, breathability, and mechanical properties. At the same time, their acid and alkali resistance stability is poor, which limits the use efficiency of the product.
Polyester fiber and carbon fiber are blended to form the first yarn, and modified polyamide fiber is spun into the second yarn. It is combined with biological enzyme washing treatment and treatment liquid immersion treatment to form a moisture-absorbing and breathable fabric. The synergistic effect of pre-conditioning liquid and strengthening agent optimizes fiber body performance, enhances interface connectivity and breathability and moisture absorption.
It achieves the coordination of moisture absorption, breathability and mechanical properties of moisture-absorbent and breathable fabrics. At the same time, it significantly improves the stability of the product in different acid and alkali environments and ensures the acid and alkali resistance of the fabric.
Smart Images

Figure BDA0004888727760000121 
Figure BDA0004888727760000131 
Figure BDA0004888727760000132
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabrics, and in particular to a moisture-absorbing and breathable fabric and a preparation method thereof. Background Art
[0002] Clothing is composed of three elements: clothing style, clothing color and clothing fabric. Among them, clothing fabric is the material used to make clothing and is the most basic element. Clothing fabric can not only interpret the style and characteristics of clothing, but also directly affect the color and shape of clothing. Generally, clothing fabrics have the characteristics of being comfortable to wear, sweat-absorbent and breathable, drapey and crisp, visually noble and soft to the touch.
[0003] Existing fabrics have poor air permeability and moisture absorption properties. In order to improve the moisture absorption and air permeability of the product, the mechanical properties of the product are prone to deterioration, making it difficult to achieve coordinated improvements in the moisture absorption and air permeability and mechanical properties of the product. In addition, the product has poor acid and alkali resistance, which further limits the product's use efficiency. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a moisture-absorbing and breathable fabric and a preparation method thereof to solve the problems raised in the above-mentioned background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides a method for preparing a moisture-absorbing and breathable fabric, comprising the following steps:
[0007] Step 1: blending polyester fiber and carbon fiber in a weight ratio of (2-3):1 to form a first yarn, and spinning modified polyamide fiber into a second yarn;
[0008] Step 2: treating the first yarn and the second yarn with biological enzyme washing respectively to obtain enzyme-washed first yarn and enzyme-washed second yarn;
[0009] The specific steps of the biological enzyme washing treatment are:
[0010] 2-5 parts by weight of cellulase, 1-3 parts of fatty alcohol polyoxyethylene ether, 1-2 parts of citric acid, 10-15 parts of ethanol solvent, and 2-4 parts of amino silicone oil are mixed to obtain an enzyme washing solution;
[0011] The first yarn and the second yarn are immersed in a sufficient amount of enzyme washing solution for 35-45 minutes at a temperature of 38-42°C. After the treatment, the yarns are washed with water and dried.
[0012] Step 3: The enzyme-washed first yarn and the enzyme-washed second yarn are used as warp yarn and weft yarn respectively, and the warp yarn and the weft yarn are woven according to a weight ratio of (1-1.5):1 to form a fabric body;
[0013] Step 4: Finally, immerse the fabric body in a sufficient amount of treatment liquid for immersion treatment. The immersion power is 300-400W and the immersion time is 1-2h. After the treatment is completed, wash and dry.
[0014] Preferably, the modification method of the modified polyamide fiber is:
[0015] S01: treating the silicon carbide whisker with proton irradiation at a power of 350-400W for 1-2h, and obtaining irradiated silicon carbide whiskers after the irradiation is completed;
[0016] S02: 1-3 parts of silane coupling agent KH560 and 2-4 parts of irradiated silicon carbide whiskers are added to 8-12 parts of 10% by mass sodium lignin sulfonate solution, and then 1-3 parts of stearic acid are added and mixed thoroughly to obtain a pre-adjusted solution;
[0017] The polyamide fiber is first placed in a sufficient amount of pre-conditioning liquid for ultrasonic pre-conditioning treatment, and after the pre-conditioning is completed, the fiber is filtered and dried to obtain the pre-conditioned polyamide fiber;
[0018] S03: Immerse the pre-adjusted polyamide fiber into a sufficient amount of strengthening agent for immersion treatment. After the treatment is completed, filter and dry.
[0019] Preferably, the ultrasonic power of the ultrasonic pre-conditioning treatment is 350-400W, and the ultrasonic time is 20-30min; the immersion pressure of the immersion treatment is 10-15MPa, the immersion time is 45-55min, and the immersion temperature is 55-60°C.
[0020] Preferably, the preparation method of the strengthening agent is:
[0021] The bentonite is first heated to 210-220°C at a rate of 2-5°C / min, kept warm for 10-15min, then heated to 350°C at a rate of 1-3°C / min, kept warm for 5min, and finally air-cooled to room temperature to obtain a bentonite agent;
[0022] Add 5-8 parts of bentonite and 2-5 parts of chitosan solution to 6-10 parts of sodium citrate solution, then add 2-5 parts of phosphate buffer solution, stir and mix thoroughly to obtain a strengthening agent.
[0023] Preferably, the mass fraction of the chitosan solution is 2-5%; the mass fraction of the sodium citrate solution is 8-12%.
[0024] Preferably, the pH value of the phosphate buffer solution is 5.0-5.5.
[0025] Preferably, the treatment solution comprises the following raw materials in parts by weight:
[0026] 2-5 parts of sodium alginate, 1-3 parts of methyl trifluoropropyl silicone oil, 4-7 parts of sodium dodecylbenzene sulfonate solution and 2-5 parts of nano silicon dioxide; wherein the preparation method of the nano silicon dioxide is:
[0027] Nano-silicon dioxide, 5% by mass lanthanum nitrate solution and magnesium chloride solution are mixed and ball-milled in a weight ratio of 3:5:2. After the ball-milling is completed, a nano-silicon dioxide agent is obtained.
[0028] Preferably, the mass fraction of the sodium dodecylbenzene sulfonate solution is 10-15%; the mass fraction of the magnesium chloride solution is 2-5%.
[0029] Preferably, the ball milling speed of the ball milling treatment is 1000-1500 r / min, the ball milling is performed for 1-2 hours, and the ball milling is completed.
[0030] The invention also provides a method for preparing a moisture-absorbing and breathable fabric and a moisture-absorbing and breathable fabric prepared by the method.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The moisture-absorbing and breathable fabric of the present invention is formed by blending polyester fiber with carbon fiber to form a first yarn, and a second yarn is spun by modified polyamide fiber. The fabric is washed with enzymes, spun and immersed in a treatment liquid to obtain a fabric with coordinated moisture absorption, breathability and mechanical properties. At the same time, the product has significant stability under different degrees of acid conditions and alkaline environments;
[0033] 2. The modified polyamide fiber is subjected to ultrasonic pre-conditioning treatment in a pre-conditioning liquid, and then improved by immersion in a strengthening agent. Silicon carbide whiskers are irradiated with protons to optimize their active performance. Then, the pre-conditioning liquid formed is adjusted and blended with silane coupling agent KH560, irradiated silicon carbide whiskers, sodium lignin sulfonate solution and stearic acid. The whiskers with whisker-like structures are used to coordinate with the raw materials in the pre-conditioning liquid to improve the fiber body, optimize the interface between the weft and the warp obtained by the polyamide fiber, enhance the interface connectivity, optimize the performance of the product, and enhance the further synergistic effect between the polyamide fiber body and the strengthening agent.
[0034] 3. The strengthening agent is bentonite, which is first heated to 210-220°C at a rate of 2-5°C / min, kept warm for 10-15 minutes, and then heated to 350°C at a rate of 1-3°C / min, and kept warm for 5 minutes, and finally air-cooled to room temperature to optimize the interlaminar spacing and activity of the bentonite. At the same time, the bentonite agent, chitosan solution, sodium citrate solution, and phosphate buffer solution are blended to obtain the strengthening agent. The interlaminar structure of the bentonite is used to optimize the spatial channel and improve the air permeability and moisture absorption of the product. At the same time, the strengthening agent and the pre-adjusting liquid are used to coordinate and prepare together, so that the moisture absorption and air permeability, mechanical properties of the product are coordinated and improved, and the acid and alkali resistance stability of the product is further improved;
[0035] 4. The treatment liquid is blended with sodium alginate, methyl trifluoropropyl silicone oil, sodium dodecylbenzene sulfonate solution and nano-silica agent. The coordination between the raw materials can enhance the interface and connection strength between the fabrics and improve the overall stability of the product. At the same time, the nano-silica agent is made by ball-milling nano-silica with lanthanum nitrate solution and magnesium chloride solution. The ball-milled nano-silica further improves the performance of the product in the treatment liquid, thereby further improving the performance of the product. DETAILED DESCRIPTION
[0036] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] A method for preparing a moisture-absorbing and breathable fabric in this embodiment comprises the following steps:
[0038] Step 1: blending polyester fiber and carbon fiber in a weight ratio of (2-3):1 to form a first yarn, and spinning modified polyamide fiber into a second yarn;
[0039] Step 2: treating the first yarn and the second yarn with biological enzyme washing respectively to obtain enzyme-washed first yarn and enzyme-washed second yarn;
[0040] The specific steps of the biological enzyme washing treatment are:
[0041] 2-5 parts by weight of cellulase, 1-3 parts of fatty alcohol polyoxyethylene ether, 1-2 parts of citric acid, 10-15 parts of ethanol solvent, and 2-4 parts of amino silicone oil are mixed to obtain an enzyme washing solution;
[0042] The first yarn and the second yarn are immersed in a sufficient amount of enzyme washing solution for 35-45 minutes at a temperature of 38-42°C. After the treatment, the yarns are washed with water and dried.
[0043] Step 3: The enzyme-washed first yarn and the enzyme-washed second yarn are used as warp yarn and weft yarn respectively, and the warp yarn and the weft yarn are woven according to a weight ratio of (1-1.5):1 to form a fabric body;
[0044] Step 4: Finally, immerse the fabric body in a sufficient amount of treatment liquid for immersion treatment. The immersion power is 300-400W and the immersion time is 1-2h. After the treatment is completed, wash and dry.
[0045] The modification method of the modified polyamide fiber of this embodiment is:
[0046] S01: treating the silicon carbide whisker with proton irradiation at a power of 350-400W for 1-2h, and obtaining irradiated silicon carbide whiskers after the irradiation is completed;
[0047] S02: 1-3 parts of silane coupling agent KH560 and 2-4 parts of irradiated silicon carbide whiskers are added to 8-12 parts of 10% by mass sodium lignin sulfonate solution, and then 1-3 parts of stearic acid are added and mixed thoroughly to obtain a pre-adjusted solution;
[0048] The polyamide fiber is first placed in a sufficient amount of pre-conditioning liquid for ultrasonic pre-conditioning treatment, and after the pre-conditioning is completed, the fiber is filtered and dried to obtain the pre-conditioned polyamide fiber;
[0049] S03: Immerse the pre-adjusted polyamide fiber into a sufficient amount of strengthening agent for immersion treatment. After the treatment is completed, filter and dry.
[0050] The ultrasonic power of the ultrasonic pre-conditioning treatment in this embodiment is 350-400W, and the ultrasonic time is 20-30min; the immersion pressure of the immersion treatment is 10-15MPa, the immersion time is 45-55min, and the immersion temperature is 55-60°C.
[0051] The preparation method of the strengthening agent of this embodiment is:
[0052] The bentonite is first heated to 210-220°C at a rate of 2-5°C / min, kept warm for 10-15min, then heated to 350°C at a rate of 1-3°C / min, kept warm for 5min, and finally air-cooled to room temperature to obtain a bentonite agent;
[0053] Add 5-8 parts of bentonite and 2-5 parts of chitosan solution to 6-10 parts of sodium citrate solution, then add 2-5 parts of phosphate buffer solution, stir and mix thoroughly to obtain a strengthening agent.
[0054] The mass fraction of the chitosan solution in this embodiment is 2-5%; the mass fraction of the sodium citrate solution is 8-12%.
[0055] The pH value of the phosphate buffer solution of this embodiment is 5.0-5.5.
[0056] The treatment solution of this embodiment includes the following raw materials in parts by weight:
[0057] 2-5 parts of sodium alginate, 1-3 parts of methyl trifluoropropyl silicone oil, 4-7 parts of sodium dodecylbenzene sulfonate solution and 2-5 parts of nano silicon dioxide; wherein the preparation method of the nano silicon dioxide is:
[0058] Nano-silicon dioxide, 5% by mass lanthanum nitrate solution and magnesium chloride solution are mixed and ball-milled in a weight ratio of 3:5:2. After the ball-milling is completed, a nano-silicon dioxide agent is obtained.
[0059] The mass fraction of the sodium dodecylbenzene sulfonate solution in this embodiment is 10-15%; the mass fraction of the magnesium chloride solution is 2-5%.
[0060] The ball milling speed of the ball milling treatment in this embodiment is 1000-1500r / min, and the ball milling is completed after 1-2h.
[0061] The present embodiment provides a method for preparing a moisture-absorbing and breathable fabric to prepare a moisture-absorbing and breathable fabric.
[0062] Example 1.
[0063] A method for preparing a moisture-absorbing and breathable fabric in this embodiment comprises the following steps:
[0064] Step 1: blending polyester fiber and carbon fiber in a weight ratio of 2:1 to form a first yarn, and spinning modified polyamide fiber into a second yarn;
[0065] Step 2: treating the first yarn and the second yarn with biological enzyme washing respectively to obtain enzyme-washed first yarn and enzyme-washed second yarn;
[0066] The specific steps of the biological enzyme washing treatment are:
[0067] 2 parts by weight of cellulase, 1 part of fatty alcohol polyoxyethylene ether, 1 part of citric acid, 10 parts of ethanol solvent and 2 parts of amino silicone oil are mixed to obtain an enzyme washing solution;
[0068] The first yarn and the second yarn are immersed in a sufficient amount of enzyme washing solution for 35 minutes at a temperature of 38°C. After the treatment, the yarns are washed with water and dried.
[0069] Step 3: The enzyme-washed first yarn and the enzyme-washed second yarn are used as warp yarn and weft yarn respectively, and the warp yarn and the weft yarn are woven according to a weight ratio of 1:1 to form a fabric body;
[0070] Step 4: Finally, immerse the fabric body in a sufficient amount of treatment liquid for immersion treatment. The immersion power is 300W and the immersion time is 1 hour. After the treatment is completed, wash and dry.
[0071] The modification method of the modified polyamide fiber of this embodiment is:
[0072] S01: treating the silicon carbide whisker with proton irradiation at a power of 350 W for 1 hour, and then obtaining irradiated silicon carbide whiskers after the irradiation is completed;
[0073] S02: 1 part of silane coupling agent KH560 and 2 parts of irradiated silicon carbide whiskers are added to 8 parts of 10% sodium lignin sulfonate solution by mass, and then 1 part of stearic acid is added and mixed thoroughly to obtain a pre-adjusted solution;
[0074] The polyamide fiber is first placed in a sufficient amount of pre-conditioning liquid for ultrasonic pre-conditioning treatment, and after the pre-conditioning is completed, the fiber is filtered and dried to obtain the pre-conditioned polyamide fiber;
[0075] S03: Immerse the pre-adjusted polyamide fiber into a sufficient amount of strengthening agent for immersion treatment. After the treatment is completed, filter and dry.
[0076] The ultrasonic power of the ultrasonic pre-conditioning treatment in this embodiment is 350W, and the ultrasonic time is 20min; the immersion pressure of the immersion treatment is 10MPa, the immersion time is 45min, and the immersion temperature is 55°C.
[0077] The preparation method of the strengthening agent of this embodiment is:
[0078] The bentonite was first heated to 210°C at a rate of 2°C / min, kept at that temperature for 10 minutes, then heated to 350°C at a rate of 1°C / min, kept at that temperature for 5 minutes, and finally air-cooled to room temperature to obtain a bentonite agent;
[0079] Add 1 part of bentonite and 2 parts of chitosan solution into 6 parts of sodium citrate solution, then add 2 parts of phosphate buffer solution, stir and mix thoroughly to obtain a strengthening agent.
[0080] The mass fraction of the chitosan solution in this embodiment is 2%; the mass fraction of the sodium citrate solution is 8%.
[0081] The pH value of the phosphate buffer solution in this example is 5.5.
[0082] The treatment solution of this embodiment includes the following raw materials in parts by weight:
[0083] 2 parts of sodium alginate, 1 part of methyl trifluoropropyl silicone oil, 4 parts of sodium dodecylbenzene sulfonate solution and 2 parts of nano silicon dioxide; wherein the preparation method of the nano silicon dioxide is:
[0084] Nano-silicon dioxide, 5% by mass lanthanum nitrate solution and magnesium chloride solution are mixed and ball-milled in a weight ratio of 3:5:2. After the ball-milling is completed, a nano-silicon dioxide agent is obtained.
[0085] The mass fraction of the sodium dodecylbenzene sulfonate solution in this embodiment is 10%; the mass fraction of the magnesium chloride solution is 2%.
[0086] The ball milling speed of the ball milling treatment in this embodiment is 1000 r / min, and the ball milling is completed after 1 hour of ball milling.
[0087] The present embodiment provides a method for preparing a moisture-absorbing and breathable fabric to prepare a moisture-absorbing and breathable fabric.
[0088] Example 2.
[0089] A method for preparing a moisture-absorbing and breathable fabric in this embodiment comprises the following steps:
[0090] Step 1: blending polyester fiber and carbon fiber in a weight ratio of 2:1 to form a first yarn, and spinning modified polyamide fiber into a second yarn;
[0091] Step 2: treating the first yarn and the second yarn with biological enzyme washing respectively to obtain enzyme-washed first yarn and enzyme-washed second yarn;
[0092] The specific steps of the biological enzyme washing treatment are:
[0093] 5 parts by weight of cellulase, 3 parts of fatty alcohol polyoxyethylene ether, 2 parts of citric acid, 15 parts of ethanol solvent and 4 parts of amino silicone oil are mixed to obtain an enzyme washing solution;
[0094] The first yarn and the second yarn are immersed in a sufficient amount of enzyme washing solution for 45 minutes at a treatment temperature of 42°C. After the treatment, the yarns are washed with water and dried;
[0095] Step 3: The enzyme-washed first yarn and the enzyme-washed second yarn are used as warp yarn and weft yarn respectively, and the warp yarn and the weft yarn are woven according to a weight ratio of 1:1 to form a fabric body;
[0096] Step 4: Finally, immerse the fabric body in a sufficient amount of treatment liquid for immersion treatment. The immersion power is 400W and the immersion time is 1 hour. After the treatment is completed, wash and dry.
[0097] The modification method of the modified polyamide fiber of this embodiment is:
[0098] S01: treating the silicon carbide whisker with proton irradiation at a power of 400 W for 2 hours, and then obtaining irradiated silicon carbide whiskers after the irradiation is completed;
[0099] S02: 3 parts of silane coupling agent KH560 and 4 parts of irradiated silicon carbide whiskers are added to 12 parts of 10% sodium lignin sulfonate solution by mass, and then 3 parts of stearic acid are added and mixed thoroughly to obtain a pre-adjusted solution;
[0100] The polyamide fiber is first placed in a sufficient amount of pre-conditioning liquid for ultrasonic pre-conditioning treatment, and after the pre-conditioning is completed, the fiber is filtered and dried to obtain the pre-conditioned polyamide fiber;
[0101] S03: Immerse the pre-adjusted polyamide fiber into a sufficient amount of strengthening agent for immersion treatment. After the treatment is completed, filter and dry.
[0102] The ultrasonic power of the ultrasonic pre-conditioning treatment in this embodiment is 400W, and the ultrasonic time is 30min; the immersion pressure of the immersion treatment is 15MPa, the immersion time is 55min, and the immersion temperature is 60°C.
[0103] The preparation method of the strengthening agent of this embodiment is:
[0104] The bentonite was first heated to 220°C at a rate of 5°C / min, kept at that temperature for 15 minutes, then heated to 350°C at a rate of 3°C / min, kept at that temperature for 5 minutes, and finally air-cooled to room temperature to obtain a bentonite agent;
[0105] 8 parts of bentonite and 5 parts of chitosan solution were added to 10 parts of sodium citrate solution, and then 5 parts of phosphate buffer solution were added, and the mixture was stirred and mixed thoroughly to obtain a strengthening agent.
[0106] The mass fraction of the chitosan solution in this embodiment is 5%; the mass fraction of the sodium citrate solution is 12%.
[0107] The pH value of the phosphate buffer solution in this example is 5.5.
[0108] The treatment solution of this embodiment includes the following raw materials in parts by weight:
[0109] 5 parts of sodium alginate, 3 parts of methyl trifluoropropyl silicone oil, 7 parts of sodium dodecylbenzene sulfonate solution and 5 parts of nano silicon dioxide; wherein the preparation method of the nano silicon dioxide is:
[0110] Nano-silicon dioxide, 5% by mass lanthanum nitrate solution and magnesium chloride solution are mixed and ball-milled in a weight ratio of 3:5:2. After the ball-milling is completed, a nano-silicon dioxide agent is obtained.
[0111] The mass fraction of the sodium dodecylbenzene sulfonate solution in this embodiment is 15%; the mass fraction of the magnesium chloride solution is 5%.
[0112] The ball milling speed of the ball milling treatment in this embodiment is 1500 r / min, and the ball milling is completed after 1 hour of ball milling.
[0113] The present embodiment provides a method for preparing a moisture-absorbing and breathable fabric to prepare a moisture-absorbing and breathable fabric.
[0114] Example 3.
[0115] A method for preparing a moisture-absorbing and breathable fabric in this embodiment comprises the following steps:
[0116] Step 1: blending polyester fiber and carbon fiber in a weight ratio of 2:1 to form a first yarn, and spinning modified polyamide fiber into a second yarn;
[0117] Step 2: treating the first yarn and the second yarn with biological enzyme washing respectively to obtain enzyme-washed first yarn and enzyme-washed second yarn;
[0118] The specific steps of the biological enzyme washing treatment are:
[0119] 3.5 parts by weight of cellulase, 2 parts of fatty alcohol polyoxyethylene ether, 1.5 parts of citric acid, 12.5 parts of ethanol solvent and 3 parts of amino silicone oil are mixed to obtain an enzyme washing solution;
[0120] The first yarn and the second yarn are immersed in a sufficient amount of enzyme washing solution for 40 minutes at a treatment temperature of 40°C. After the treatment, the yarns are washed with water and dried;
[0121] Step 3: The enzyme-washed first yarn and the enzyme-washed second yarn are used as warp yarn and weft yarn respectively, and the warp yarn and the weft yarn are woven according to a weight ratio of 1:1 to form a fabric body;
[0122] Step 4: Finally, immerse the fabric body in a sufficient amount of treatment liquid for immersion treatment. The immersion power is 350W and the immersion time is 1 hour. After the treatment is completed, wash and dry.
[0123] The modification method of the modified polyamide fiber of this embodiment is:
[0124] S01: treating the silicon carbide whisker with proton irradiation at a power of 370 W for 1.5 h, and obtaining irradiated silicon carbide whiskers after the irradiation is completed;
[0125] S02: 2 parts of silane coupling agent KH560 and 3 parts of irradiated silicon carbide whiskers are added to 10 parts of 10% sodium lignin sulfonate solution by mass, and then 2 parts of stearic acid are added and mixed thoroughly to obtain a pre-adjusted solution;
[0126] The polyamide fiber is first placed in a sufficient amount of pre-conditioning liquid for ultrasonic pre-conditioning treatment, and after the pre-conditioning is completed, the fiber is filtered and dried to obtain the pre-conditioned polyamide fiber;
[0127] S03: Immerse the pre-adjusted polyamide fiber into a sufficient amount of strengthening agent for immersion treatment. After the treatment is completed, filter and dry.
[0128] The ultrasonic power of the ultrasonic pre-conditioning treatment in this embodiment is 370W, and the ultrasonic time is 25min; the immersion pressure of the immersion treatment is 12.5MPa, the immersion time is 50min, and the immersion temperature is 57°C.
[0129] The preparation method of the strengthening agent of this embodiment is:
[0130] The bentonite was first heated to 215°C at a rate of 3.5°C / min, kept at that temperature for 12.5min, then heated to 350°C at a rate of 2°C / min, kept at that temperature for 5min, and finally cooled to room temperature in air to obtain a bentonite agent;
[0131] 6.5 parts of bentonite and 3.5 parts of chitosan solution were added to 8 parts of sodium citrate solution, and then 3.5 parts of phosphate buffer solution were added, and the mixture was stirred and mixed thoroughly to obtain a strengthening agent.
[0132] The mass fraction of the chitosan solution in this embodiment is 3.5%; the mass fraction of the sodium citrate solution is 10%.
[0133] The pH value of the phosphate buffer solution in this example is 5.5.
[0134] The treatment solution of this embodiment includes the following raw materials in parts by weight:
[0135] 3.5 parts of sodium alginate, 2 parts of methyl trifluoropropyl silicone oil, 5.5 parts of sodium dodecylbenzene sulfonate solution and 3.5 parts of nano silicon dioxide; wherein the preparation method of the nano silicon dioxide is:
[0136] Nano-silicon dioxide, 5% by mass lanthanum nitrate solution and magnesium chloride solution are mixed and ball-milled in a weight ratio of 3:5:2. After the ball-milling is completed, a nano-silicon dioxide agent is obtained.
[0137] The mass fraction of the sodium dodecylbenzene sulfonate solution in this embodiment is 12.5%; the mass fraction of the magnesium chloride solution is 3.5%.
[0138] The ball milling speed of the ball milling treatment in this embodiment is 1250 r / min, and the ball milling is completed after 1 hour of ball milling.
[0139] The present embodiment provides a method for preparing a moisture-absorbing and breathable fabric to prepare a moisture-absorbing and breathable fabric.
[0140] Comparative Example 1.
[0141] The difference from Example 3 is that the modified polyamide fiber is replaced by polyamide fiber.
[0142] Comparative Example 2.
[0143] The difference from Example 3 is that no pre-adjusting liquid treatment is used in the modification of the modified polyamide fiber.
[0144] Comparative Example 3.
[0145] The difference from Example 3 is that no silane coupling agent KH560 and irradiated silicon carbide whiskers are added to the pre-adjusted liquid.
[0146] Comparative Example 4.
[0147] The difference from Example 3 is that no strengthening agent is used in the modification of the modified polyamide fiber.
[0148] Comparative Example 5.
[0149] The difference from Example 3 is that no bentonite is added to the strengthening agent.
[0150] Comparative Example 6.
[0151] The difference from Example 3 is that the bentonite agent is directly replaced by the bentonite raw material.
[0152] Comparative Example 7.
[0153] The difference from Example 3 is that no treatment liquid is used for treatment.
[0154] Comparative Example 8.
[0155] The difference from Example 3 is that no nano-silicon dioxide agent is added to the treatment liquid.
[0156] Comparative Example 9.
[0157] The difference from Example 3 is that the nano-silica agent is not ball-milled with lanthanum nitrate solution and magnesium chloride solution.
[0158] The products of Examples 1-3 and Comparative Examples 1-9 were tested under normal conditions:
[0159] The performance measurement results are as follows
[0160]
[0161]
[0162] It can be concluded from Examples 1-3 and Comparative Examples 1-9 that
[0163] The products of Examples 1-3 have excellent breaking strength, air permeability and moisture permeability, and the air permeability, moisture permeability and mechanical properties of the products can be improved in a coordinated manner. The product performances of Examples 1-3 are significantly better than those of Comparative Examples 1-9.
[0164] The product was placed in an acidic environment of pH 3.0, pH 6.0 and an alkaline environment of pH 10.0 for 5 days and then the mechanical, air and moisture permeability stability of the product was tested. The acid and alkali stability of the product was tested in acidic and alkaline environments of different degrees. The test results are as follows:
[0165]
[0166]
[0167] The product of Example 3 of the present invention has significant stability effects on mechanical properties and moisture permeability and air permeability in acidic environments of pH 3.0 and pH 6.0 and in alkaline environments of pH 10.0;
[0168] It can be seen from Comparative Examples 1-9 and Example 3 that when the modified polyamide fiber is replaced by polyamide fiber and not treated with the treatment liquid, the performance stability of the product is significantly deteriorated, and the stability of the product is significantly deteriorated in acidic and alkaline environments of different degrees. The modified polyamide fiber of the present invention is used in combination with the treatment liquid for treatment, and the two are synergistically enhanced, and the performance effect of the product is significant;
[0169] The modified polyamide fiber modification does not use pre-adjustment liquid treatment, does not add silane coupling agent KH560 and irradiated silicon carbide whiskers in the pre-adjustment liquid, does not use strengthening agent treatment in the modified polyamide fiber modification, does not add bentonite agent in the strengthening agent, and the bentonite agent is directly replaced by bentonite raw materials. The performance of the product has a tendency to deteriorate. The pre-adjustment liquid and the modified polyamide fiber modified by the strengthening agent obtained by the method of the present invention have the most significant performance effect of the product. The effect of using other methods instead is not as obvious as that of the present invention. At the same time, no nano-silica agent is added to the treatment liquid, and the nano-silica agent is not ball-milled with lanthanum nitrate solution and magnesium chloride solution. The performance of the product has a tendency to deteriorate. Only the treatment liquid prepared by the nano-silica agent obtained by the method of the present invention has the most significant performance effect of the product. The effect of using other methods instead is not as obvious as that of the present invention.
[0170] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0171] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for preparing a moisture-absorbing and breathable fabric, characterized in that: The following steps are involved: Step 1: blending polyester fiber and carbon fiber in a weight ratio of (2-3):1 to form a first yarn, and spinning modified polyamide fiber into a second yarn; Step 2: treating the first yarn and the second yarn with biological enzyme washing respectively to obtain enzyme-washed first yarn and enzyme-washed second yarn; The specific steps of the biological enzyme washing treatment are: 2-5 parts by weight of cellulase, 1-3 parts of fatty alcohol polyoxyethylene ether, 1-2 parts of citric acid, 10-15 parts of ethanol solvent, and 2-4 parts of amino silicone oil are mixed to obtain an enzyme washing solution; The first yarn and the second yarn are immersed in a sufficient amount of enzyme washing solution for 35-45 minutes at a temperature of 38-42°C. After the treatment, the yarns are washed with water and dried. Step 3: The enzyme-washed first yarn and the enzyme-washed second yarn are used as warp yarn and weft yarn respectively, and the warp yarn and the weft yarn are woven according to a weight ratio of (1-1.5):1 to form a fabric body; Step 4: Finally, immerse the fabric body in a sufficient amount of treatment liquid for immersion treatment. The immersion power is 300-400W and the immersion time is 1-2h. After the treatment is completed, wash and dry.
2. The method for preparing a moisture-absorbing and breathable fabric according to claim 1, characterized in that: The modification method of the modified polyamide fiber is: S01: treating the silicon carbide whisker with proton irradiation at a power of 350-400W for 1-2h, and obtaining irradiated silicon carbide whiskers after the irradiation is completed; S02: 1-3 parts of silane coupling agent KH560 and 2-4 parts of irradiated silicon carbide whiskers are added to 8-12 parts of 10% by mass sodium lignin sulfonate solution, and then 1-3 parts of stearic acid are added and mixed thoroughly to obtain a pre-adjusted solution; The polyamide fiber is first placed in a sufficient amount of pre-conditioning liquid for ultrasonic pre-conditioning treatment, and after the pre-conditioning is completed, the fiber is filtered and dried to obtain the pre-conditioned polyamide fiber; S03: Immerse the pre-adjusted polyamide fiber into a sufficient amount of strengthening agent for immersion treatment. After the treatment is completed, filter and dry.
3. The method for preparing a moisture-absorbing and breathable fabric according to claim 2, characterized in that: The ultrasonic power of the ultrasonic pre-adjustment treatment is 350-400W, and the ultrasonic time is 20-30min; the immersion pressure of the immersion treatment is 10-15MPa, the immersion time is 45-55min, and the immersion temperature is 55-60°C.
4. The method for preparing a moisture-absorbing and breathable fabric according to claim 2, characterized in that: The preparation method of the strengthening agent is: The bentonite is first heated to 210-220°C at a rate of 2-5°C / min, kept warm for 10-15min, then heated to 350°C at a rate of 1-3°C / min, kept warm for 5min, and finally air-cooled to room temperature to obtain a bentonite agent; Add 5-8 parts of bentonite and 2-5 parts of chitosan solution to 6-10 parts of sodium citrate solution, then add 2-5 parts of phosphate buffer solution, stir and mix thoroughly to obtain a strengthening agent.
5. The method for preparing a moisture-absorbing and breathable fabric according to claim 4, characterized in that: The mass fraction of the chitosan solution is 2-5%; the mass fraction of the sodium citrate solution is 8-12%.
6. The method for preparing a moisture-absorbing and breathable fabric according to claim 4, characterized in that: The pH value of the phosphate buffer solution is 5.0-5.
5.
7. The method for preparing a moisture-absorbing and breathable fabric according to claim 1, characterized in that: The treatment solution comprises the following raw materials in parts by weight: 2-5 parts of sodium alginate, 1-3 parts of methyl trifluoropropyl silicone oil, 4-7 parts of sodium dodecylbenzene sulfonate solution and 2-5 parts of nano silicon dioxide; wherein the preparation method of the nano silicon dioxide is: Nano-silicon dioxide, 5% by mass lanthanum nitrate solution and magnesium chloride solution are mixed and ball-milled in a weight ratio of 3:5:
2. After the ball-milling is completed, a nano-silicon dioxide agent is obtained.
8. The method for preparing a moisture-absorbing and breathable fabric according to claim 7, characterized in that: The mass fraction of the sodium dodecylbenzene sulfonate solution is 10-15%; the mass fraction of the magnesium chloride solution is 2-5%.
9. The method for preparing a moisture-absorbing and breathable fabric according to claim 7, characterized in that: The ball milling speed of the ball milling treatment is 1000-1500r / min, and the ball milling is performed for 1-2h, and the ball milling is completed.
10. A moisture-absorbing and breathable fabric prepared by the method for preparing a moisture-absorbing and breathable fabric according to any one of claims 1 to 9.
Citation Information
Patent Citations
Production method for quick-dry fabric
CN113106746A
Moisture-absorbing and heating finishing agent, preparation method and application
CN113293619A
Moisture-absorbing and quick-drying bio-based chinlon fabric and application thereof in underwear
CN115648759A
Special PVC thermoplastic elastomer cable material and preparation method thereof
CN117487295A
Waterproof breathable decorative panel material and preparation method thereof
CN117776656A
Cited By
Efficient moisture absorption and sweat releasing knitted fabric and preparation method thereof