Protective fabric for fencing suit and preparation method of protective fabric

By using graphene-modified polyurethane solution on aramid fiber fabrics for impregnation treatment, the protective and conductive properties of fencing clothing are improved, the problems of lightweight and insufficient protective properties of fencing clothing in the existing technology are solved, and high-strength, Balance of conductivity and comfort.

CN118792893APending Publication Date: 2024-10-18WUXI WEIHAO SPORTS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410894039.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing protective fabrics for fencing clothing have shortcomings in terms of lightweight, protective strength, flexibility and comfort, and it is difficult to balance the lightness and durability of conductive fabrics.

Method used

Using aramid fiber as the base fabric, it is impregnated with graphene-modified polyurethane solution to improve the puncture resistance and conductivity of the fabric. The coating amount and drying conditions are controlled through the padding process to enhance the adhesion and protection of the fabric. performance.

Benefits of technology

The prepared fencing uniform has excellent protective properties and conductive properties, is light in weight, has good toughness, is comfortable to wear, and has high sword touch sensitivity, and is suitable for the technical needs of fencers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a protective fabric for fencing clothes and a preparation method thereof, and relates to the technical field of textile, the preparation method comprises the following steps: cleaning and pretreating aramid fibers, then preparing an aramid fabric, dipping the aramid fabric in a graphene modified polyurethane solution, washing with water, drying to obtain a modified aramid fabric, cutting and sewing to obtain the protective fabric for fencing clothes. The protective fabric is prepared; the prepared fencing suit has excellent protection performance and conductivity, is light in weight, good in toughness, comfortable to wear and high in fencing trigger sensitivity, and is beneficial to exerting the fencing technical level of athletes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to a protective fabric for fencing clothing and a preparation method thereof. Background Art

[0002] Since fencing became a competition sport in 1896, it has become more and more popular, and the number of participants has shown an explosive growth in recent years. For this reason, the research and development of fencing protective clothing has also received more and more attention. At the same time, the advancement of fencing protective clothing technology has also become an important boost to the steady development of fencing, a high-risk, highly confrontational competitive sport.

[0003] At present, the protective clothing and conductive clothing of fencing sportswear are separated. Protective clothing is used to prevent potential threats in fencing, protect the human body, and greatly reduce the danger of this sport. The requirements for puncture strength of protective fabrics are very high. The average force of the anti-puncture standard of the second-level fencing clothing should be greater than or equal to 800N. The fencing fabrics currently used in the market are mainly made of metal wire, high-strength acrylic and cotton. Some anti-puncture fabrics use aramid fibers.

[0004] The outermost conductive clothing mainly ensures that it can timely, effectively and accurately judge whether the fencing touches the effective parts of the body. At present, the conductive fabrics produced at home and abroad are all interwoven with synthetic yarns and metal wires (mainly copper wires), which have good conductivity, but this kind of fabric is not light enough, has a hard texture, and is not soft enough. In addition, the metal wires are easily oxidized when they are damp during use. The generated oxides (such as verdigris) not only affect the conductive properties of the conductive clothing, but also cause great harm to the wearer's skin and respiratory system. There are many disadvantages of the currently known textile materials coated with inherently conductive polymers. The ideal conductive textile should contain electronic components seamlessly integrated into the conventional textile structure, have stable electrical properties, withstand normal wear and tear, and be washable and iron-resistant. At present, there are no textiles coated with conductive polymers on the market that can meet all the above requirements.

[0005] Chinese patent document CN201485573U discloses a nickel-manganese conductive wire and a fencing cloth composed of the nickel-manganese conductive wire, wherein nickel and manganese are densely wound on the teron wire, and the nickel-manganese conductive wires are distributed on the cloth in a staggered manner in warp and weft. The cloth is composed of warp and weft yarns between the two nickel-manganese conductive wires. Although this type of fencing cloth has good corrosion resistance, high strength, strong conductivity, and high sensitivity, the nickel-manganese conductive wires constituting the fencing cloth are densely wound on the teron wire, so the diameter is thick, the woven cloth is thick, and the cloth is heavy, which directly leads to the thick and heavy fencing suits made, which is cumbersome to wear, and is not conducive to the technical level of fencing athletes.

[0006] Fencing protective clothing should provide satisfactory light weight, high strength, conductivity, and good softness and comfort. Based on these requirements, some products have been promoted and applied commercially. However, with the development of competitive sports, people's performance requirements for fencing protective clothing are getting higher and higher, and higher demands are put forward for the protection and comfort of clothing. In the existing technology, fencing clothing still has deficiencies in light weight, protective strength, flexibility and comfort. Summary of the invention

[0007] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a protective fabric for fencing clothing and a preparation method thereof. The prepared fencing clothing has excellent protective performance and conductive performance, is light in weight, has good toughness, is comfortable to wear, has high sword touch trigger sensitivity, and is conducive to the athletes' display of fencing skills.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] A method for preparing a protective fabric for fencing clothing comprises the following steps: preparing an aramid fabric from aramid fiber, dipping the aramid fabric in a graphene-modified polyurethane solution, washing and drying to obtain the modified aramid fabric, cutting and sewing to obtain the protective fabric for fencing clothing.

[0010] Preferably, the method further includes a pretreatment step of the aramid fiber: washing the aramid fiber to remove surface grease, placing the aramid fiber in a NaOH solution, stirring the reaction, filtering the product, washing with water, and drying the product to obtain the pretreated aramid fiber; the concentration of the NaOH solution is 1 to 4 wt%, and the ratio of the aramid fiber to the NaOH solution is 10 g: 50 to 100 mL; and the stirring reaction conditions are stirring the reaction at 35 to 55° C. for 1 to 3 hours.

[0011] Specifically, the usage ratio of aramid fiber to NaOH solution can be 10g:50mL, 10g:60mL, 10g:70mL, 10g:80mL, 10g:90mL, 10g:100mL;

[0012] Specifically, the stirring reaction conditions can be 35° C., 40° C., 45° C., 50° C., or 55° C. for 1 h, 1.5 h, 2 h, 2.5 h, or 3 h.

[0013] Preferably, the aramid fabric is impregnated by a dip-padding process to control the coating amount to 10-25 g / cm 2 , then dry at 80-100°C for 5-20 minutes, then heat to 120-140°C and heat cure for 2-4 hours.

[0014] It is understood that the coating amount can be 10g / cm 2 , 15g / cm2 , 20g / cm 2 , 25g / cm 2 The drying conditions can be 80℃, 85℃, 90℃, 95℃, 100℃ for 5min, 10min, 15min, 20min, then heating to 120℃, 125℃, 130℃, 135℃, 140℃, and heat curing for 2h, 2.5h, 3h, 3.5h, 4h.

[0015] Preferably, the method for preparing the graphene-modified polyurethane solution comprises the following steps:

[0016] (1) adding graphene to an ethanol / water solution, then dropwise adding KH570, ultrasonically treating, centrifuging, washing with alcohol, and drying the product to obtain double-bond modified graphene;

[0017] The structural formula of the double bond modified graphene is as follows:

[0018]

[0019] (2) adding the double bond modified graphene to DMF, then adding 2-mercaptoaniline and stirring to fully dissolve, adding methyl benzoylformate, reacting under ultraviolet light irradiation, filtering, washing, and drying the product to obtain aniline graphene;

[0020] The structural formula of the aniline graphene is as follows:

[0021]

[0022] (3) dispersing aniline graphene and dihydroxyethylglycine in DMF, ultrasonically treating, adding p-toluenesulfonic acid, heating for reaction, centrifuging the product, and washing with acetone to obtain dihydroxyethyl graphene;

[0023] The structural formula of the dihydroxyethylated graphene is as follows:

[0024]

[0025] (4) The polycarbonate diol is vacuum dehydrated, mixed evenly with isophorone diisocyanate, dihydroxyethylated graphene and acetone, nitrogen is continuously introduced, dibutyltin dilaurate is added dropwise, the temperature is increased for reaction, and after the reaction is completed, the temperature is lowered to room temperature, diluted with acetone, and then 2,2-dihydroxymethylpropionic acid is added to continue the reaction, and finally triethylamine is added for neutralization to obtain a graphene-modified polyurethane solution.

[0026] Preferably, in step (1), the ethanol / water solution is obtained by mixing ethanol and water in a volume ratio of 2 to 5:1; the mass ratio of graphene, ethanol / water solution, and KH570 is 10:80 to 120:1 to 4; and the ultrasonic treatment conditions are room temperature and ultrasonic treatment for 3 to 6 hours.

[0027] Specifically, in step (1), the volume ratio of ethanol to water in the ethanol / water solution can be 2:1, 3:1, 4:1, or 5:1; the mass ratio of graphene, ethanol / water solution, and KH570 can be 10:80:1, 10:90:1, 10:100:1, 10:110:1, 10:120:1, 10:80:2, 10:90:2, 10:100:2, 10:110:2, 10:120:2, 10:80:3, 10:90:3, 10:100:3, 10:110:3, 10:120:3, 10:80:4, 10:90:4, 10:100:4, 10:110:4, or 10:120:4; and the ultrasonic treatment conditions are room temperature and ultrasonic treatment for 3 h, 4 h, 5 h, or 6 h.

[0028] Preferably, in step (2), the mass ratio of double bond modified graphene, 2-mercaptoaniline and methyl benzoylformate is 10:8.34-15.56:0.3-1.

[0029] Preferably, in step (2), the wavelength of the ultraviolet light is 365 nm, and the radiation power is 10 to 50 mW / cm 2 , irradiation time 20 to 40 minutes.

[0030] Specifically, in step (2), the wavelength of the ultraviolet light is 365 nm, and the radiation power can be 10 mW / cm 2 , 20mW / cm 2 、30mW / cm 2 , 40mW / cm 2 、50mW / cm 2 The irradiation time can be 20min, 25min, 30min, 35min, or 40min.

[0031] Preferably, in step (3), the mass ratio of aniline graphene, dihydroxyethylglycine and p-toluenesulfonic acid is 10:15-30:0.5-3.

[0032] Preferably, in step (3), the heating reaction condition is 80-110° C. and stirring the reaction for 10-18 hours.

[0033] Specifically, in step (3), the heating reaction conditions can be 80, 90, 100, 110° C. and stirring the reaction for 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h.

[0034] Preferably, in step (4), the mass ratio of polycarbonate diol, isophorone diisocyanate, dihydroxyethylated graphene, dibutyltin dilaurate, and 2,2-dihydroxymethylpropionic acid is 500:200-300:10:0.5-3:10-30.

[0035] Preferably, in step (4), the temperature is raised to 60-75° C. for 4-7 h; and the continued reaction is carried out at 35-45° C. for 1-2 h.

[0036] Specifically, in step (4), the temperature reaction conditions are to heat the reaction to 60°C, 65°C, 70°C, 75°C for 4h, 5h, 6h, 7h; the continued reaction conditions are to react at 35°C, 40°C, 45°C for 1h, 1.5h, 2h.

[0037] The present invention also claims to protect a protective fabric for fencing clothing prepared by the preparation method.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1) The present invention provides a protective fabric for fencing clothing, which uses aramid fabric as a base fabric, has certain mechanical strength, elastic recovery ability and protective effect, and uses graphene-modified polyurethane solution to impregnate the protective fabric. The modified graphene can be filled in the gaps between the fabric yarns, which greatly improves the puncture resistance and strength of the fabric. The graphene and the protective fabric have good adhesion and are not easy to fall off even after long-term high-intensity use. In addition, aniline graphene also has excellent conductive properties, so that the aramid protective clothing can have excellent protective performance and conductive properties at the same time. The integrated design of the protective clothing and the conductive clothing can make the fencing clothing light in weight, easy to wear, small in overall thickness, relatively improved in flexibility, easy to dissipate heat and perspiration, making it more comfortable for athletes to wear, which is conducive to the technical level of fencing athletes.

[0040] 2) The present invention provides a graphene-modified polyurethane solution. First, graphene is treated with KH570 to reduce the surface energy of graphene so that it can be better dispersed in a solvent, and double bonds are introduced into the surface of graphene so that it can participate in a subsequent click reaction. Subsequently, under ultraviolet light irradiation and the action of a photoinitiator, methyl benzoylformate, the double bonds on the surface of the double-bond-modified graphene react with the mercapto-ene of 2-mercaptoaniline to introduce aniline functional groups into the surface of graphene. The aniline groups can synergistically improve the conductive efficiency of graphene, so that an efficient electron flow network is formed on the surface of aramid fibers. Then, p-toluenesulfonic acid is used as a catalyst to cause an amidation reaction between the amino groups on the surface of the anilinated graphene and the hydroxyl groups of dihydroxyethylglycine, so that abundant dihydroxyethyl functional groups and amide bonds are introduced into the surface of the graphene. Finally, the dihydroxyethyl functional groups are used to form a polyurethane solution. As the polymerization site of the diol monomer, it undergoes graft copolymerization with polycarbonate diol and isophorone diisocyanate, so that the polyurethane undergoes in situ polymerization on the graphene surface to obtain graphene-modified polyurethane, which can improve the dispersibility of graphene in polyurethane and significantly improve the crosslinking degree and mechanical strength of polyurethane; subsequently, the graphene-modified polyurethane solution is coated on the surface of the aramid fabric through a dip-rolling process. The flexible molecular chains contained in the polyurethane can provide excellent bending and impact resistance, and give the aramid fabric better puncture resistance. The modified graphene nanoparticles are embedded in the surface of the aramid fabric after curing, which can further increase the mechanical strength of the protective fabric and improve the puncture resistance of the fabric. In addition, it can also give the aramid fiber excellent conductive properties, so that the prepared fencing suit is light, flexible, conductive, and has high sword touch trigger sensitivity. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.

[0042] Unless otherwise specified, the chemical reagents and materials in the present invention are purchased from commercial sources or synthesized from raw materials purchased from commercial sources.

[0043] The polycarbonate diol was purchased from Nantong Runfeng Petrochemical Co., Ltd. with the brand name UH-CARB50.

[0044] The isophorone diisocyanate is a mixture of 75% cis-isomers and 25% trans-isomers, and its model number is Desmodur I from Covestro (formerly Bayer).

[0045] A method for preparing a protective fabric for fencing clothing comprises the following steps:

[0046] (1) adding 10 g of graphene to 80-120 g of ethanol / water solution (ethanol and water are mixed in a volume ratio of 2-5:1), then dropping 1-4 g of KH570, treating at room temperature and under ultrasonic action for 3-6 h, centrifuging the product, washing with alcohol, and drying to obtain double-bond modified graphene;

[0047] (2) 10 g of double bond modified graphene was added to 100 mL of DMF, and then 8.34-15.56 g of 2-mercaptoaniline was added and stirred to fully dissolve, and 0.3-1 g of methyl benzoylformate was added. The mixture was then irradiated with ultraviolet light at a wavelength of 365 nm and a radiation power of 10-50 mW / cm 2 The product is irradiated and reacted for 20 to 40 minutes, and filtered, washed, and dried to obtain aniline graphene;

[0048] (3) dispersing 10 g of aniline graphene and 15-30 g of dihydroxyethylglycine in DMF, ultrasonically treating, adding 0.5-3 g of p-toluenesulfonic acid, stirring and reacting at 80-110° C. for 10-18 h, centrifuging the product, and washing with acetone to obtain dihydroxyethylated graphene;

[0049] (4) 500 g of polycarbonate diol was vacuum dehydrated, mixed evenly with 200-300 g of isophorone diisocyanate, 10 g of dihydroxyethylated graphene and acetone, nitrogen was continuously introduced, 0.5-3 g of dibutyltin dilaurate was added dropwise, the temperature was raised to 60-75° C. and reacted for 4-7 h. After the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 10-30 g of 2,2-dihydroxymethylpropionic acid was added, and the reaction was continued at 35-45° C. for 1-2 h. Finally, triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0050] (5) 10 g of aramid fiber was washed to remove surface grease, placed in 50-100 mL of 1-4 wt% NaOH solution, stirred and reacted at 35-55° C. for 1-3 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0051] (6) Preparing aramid fabrics using pretreated aramid fibers, immersing the aramid fabrics in a graphene-modified polyurethane solution, and treating the aramid fabrics by a dip-rolling process, controlling the coating amount to 10 to 25 g / cm 2 , then dried at 80-100° C. for 5-20 min, then heated to 120-140° C., thermally cured for 2-4 h, washed and dried to obtain modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0052] The present invention will be further described below through specific embodiments.

[0053] Example 1

[0054] A method for preparing a protective fabric for fencing clothing comprises the following steps:

[0055] (1) 10 g of graphene was added to 120 g of ethanol / water solution (ethanol and water were mixed in a volume ratio of 5:1), and then 4 g of KH570 was added dropwise, and the mixture was treated at room temperature and under ultrasonic action for 6 h. The product was centrifuged, washed with alcohol, and dried to obtain double-bond modified graphene;

[0056] (2) 10 g of double bond modified graphene was added to 100 mL of DMF, and then 15.56 g of 2-mercaptoaniline was added and stirred to fully dissolve, and 1 g of methyl benzoylformate was added. The mixture was then irradiated with ultraviolet light at a wavelength of 365 nm and a radiation power of 50 mW / cm 2 The reaction was irradiated for 40 min, and the product was filtered, washed, and dried to obtain aniline graphene;

[0057] (3) Dispersing 10 g of aniline graphene and 30 g of dihydroxyethylglycine in DMF, ultrasonically treating, adding 3 g of p-toluenesulfonic acid, stirring and reacting at 110° C. for 18 h, centrifuging the product, and washing with acetone to obtain dihydroxyethyl graphene;

[0058] (4) 500 g of polycarbonate diol was vacuum dehydrated, mixed evenly with 300 g of isophorone diisocyanate, 10 g of dihydroxyethylated graphene and 2000 mL of acetone, nitrogen was continuously introduced, 3 g of dibutyltin dilaurate was added dropwise, the temperature was raised to 75 ° C. and reacted for 4 h. After the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 30 g of 2,2-dihydroxymethylpropionic acid was added. The reaction was continued at 45 ° C. for 2 h, and finally triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0059] (5) 10 g of 250D aramid fiber was washed to remove surface grease, placed in 100 mL of 3 wt% NaOH solution, stirred and reacted at 40° C. for 2 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0060] (6) Preparing aramid fabric using pretreated aramid fiber, immersing the aramid fabric in graphene-modified polyurethane solution, and treating it by dip-rolling process, controlling the coating amount to 25 g / cm 2 , then dried at 80°C for 10 minutes, then heated to 120°C, thermally cured for 2 hours, washed and dried to obtain the modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0061] Example 2

[0062] (1) 10 g of graphene was added to 1100 g of ethanol / water solution (ethanol and water were mixed in a volume ratio of 4:1), and then 3 g of KH570 was added dropwise, and the mixture was treated at room temperature and under ultrasonic action for 5 h. The product was centrifuged, washed with alcohol, and dried to obtain double-bond modified graphene;

[0063] (2) 10 g of double bond modified graphene was added to 100 mL of DMF, and then 13.26 g of 2-mercaptoaniline was added and stirred to fully dissolve, and 0.8 g of methyl benzoylformate was added. The mixture was then irradiated with ultraviolet light at a wavelength of 365 nm and a radiation power of 40 mW / cm 2 The reaction was irradiated for 30 min, and the product was filtered, washed, and dried to obtain aniline graphene;

[0064] (3) 10 g of aniline graphene and 25 g of dihydroxyethylglycine were dispersed in DMF, ultrasonically treated, 2.5 g of p-toluenesulfonic acid was added, and the mixture was stirred at 100° C. for 16 h. The product was centrifuged and washed with acetone to obtain dihydroxyethyl graphene;

[0065] (4) 500 g of polycarbonate diol was vacuum dehydrated, mixed evenly with 280 g of isophorone diisocyanate, 10 g of dihydroxyethylated graphene and 2000 mL of acetone, nitrogen was continuously introduced, 2.5 g of dibutyltin dilaurate was added dropwise, the temperature was raised to 70° C. and reacted for 5 h. After the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 25 g of 2,2-dihydroxymethylpropionic acid was added. The reaction was continued at 40° C. for 1.5 h, and finally triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0066] (5) 10 g of 250D aramid fiber was washed to remove surface grease, placed in 100 mL of 3 wt% NaOH solution, stirred and reacted at 40° C. for 2 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0067] (6) Preparing aramid fabric using pretreated aramid fiber, immersing the aramid fabric in graphene-modified polyurethane solution, and treating it by dip-rolling process, controlling the coating amount to 20 g / cm 2 , then dried at 90°C for 10 minutes, then heated to 130°C, thermally cured for 3 hours, washed and dried to obtain the modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0068] Example 3

[0069] (1) 10 g of graphene was added to 100 g of ethanol / water solution (ethanol and water were mixed in a volume ratio of 3:1), and then 2 g of KH570 was added dropwise, and the mixture was treated at room temperature and under ultrasonication for 4 h. The product was centrifuged, washed with alcohol, and dried to obtain double-bond modified graphene;

[0070] (2) 10 g of double bond modified graphene was added to 100 mL of DMF, and then 10.76 g of 2-mercaptoaniline was added and stirred to fully dissolve, and 0.5 g of methyl benzoylformate was added. The mixture was then irradiated with ultraviolet light at a wavelength of 365 nm and a radiation power of 300 mW / cm 2 The reaction was irradiated for 25 min, and the product was filtered, washed, and dried to obtain aniline graphene;

[0071] (3) Dispersing 10 g of aniline graphene and 20 g of dihydroxyethylglycine in DMF, ultrasonically treating, adding 1 g of p-toluenesulfonic acid, stirring and reacting at 90° C. for 12 h, centrifuging the product, and washing with acetone to obtain dihydroxyethyl graphene;

[0072] (4) 500 g of polycarbonate diol was vacuum dehydrated, mixed evenly with 220 g of isophorone diisocyanate, 10 g of dihydroxyethylated graphene and 2000 mL of acetone, nitrogen was continuously introduced, 1 g of dibutyltin dilaurate was added dropwise, the temperature was raised to 65 ° C for reaction for 6 h, and after the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 20 g of 2,2-dihydroxymethylpropionic acid was added, and the reaction was continued at 40 ° C for 1.5 h, and finally triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0073] (5) 10 g of 250D aramid fiber was washed to remove surface grease, placed in 100 mL of 3 wt% NaOH solution, stirred and reacted at 40° C. for 2 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0074] (6) Preparing aramid fabric using pretreated aramid fiber, immersing the aramid fabric in graphene-modified polyurethane solution, and treating it by dip-rolling process, controlling the coating amount to 15 g / cm 2 , then dried at 90°C for 15 minutes, then heated to 130°C, thermally cured for 3 hours, washed and dried to obtain the modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0075] Example 4

[0076] (1) 10 g of graphene was added to 80 g of ethanol / water solution (ethanol and water were mixed in a volume ratio of 2:1), and then 1 g of KH570 was added dropwise, and the mixture was treated at room temperature and under ultrasonic action for 3 h. The product was centrifuged, washed with alcohol, and dried to obtain double-bond modified graphene;

[0077] (2) 10 g of double bond modified graphene was added to 100 mL of DMF, and then 8.34 g of 2-mercaptoaniline was added and stirred to fully dissolve, and 0.3 g of methyl benzoylformate was added. The mixture was then irradiated with ultraviolet light at a wavelength of 365 nm and a radiation power of 10 mW / cm 2The reaction was irradiated for 20 min, and the product was filtered, washed, and dried to obtain aniline graphene;

[0078] (3) Dispersing 10 g of aniline graphene and 15 g of dihydroxyethylglycine in DMF, ultrasonically treating, adding 0.5 g of p-toluenesulfonic acid, stirring and reacting at 80° C. for 10 h, centrifuging the product, and washing with acetone to obtain dihydroxyethyl graphene;

[0079] (4) 500 g of polycarbonate diol was vacuum dehydrated, mixed evenly with 200 g of isophorone diisocyanate, 10 g of dihydroxyethylated graphene and 2000 mL of acetone, nitrogen was continuously introduced, 0.5 g of dibutyltin dilaurate was added dropwise, the temperature was raised to 60 ° C and reacted for 7 h, after the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 10 g of 2,2-dihydroxymethylpropionic acid was added, the reaction was continued at 35 ° C for 2 h, and finally triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0080] (5) 10 g of 250D aramid fiber was washed to remove surface grease, placed in 100 mL of 3 wt% NaOH solution, stirred and reacted at 40° C. for 2 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0081] (6) Preparing aramid fabric using pretreated aramid fiber, immersing the aramid fabric in graphene-modified polyurethane solution, and treating it by dip-rolling process, controlling the coating amount to 10 g / cm 2 , then dried at 90°C for 15 minutes, then heated to 130°C, thermally cured for 3 hours, washed and dried to obtain the modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0082] Comparative Example 1

[0083] A method for preparing a protective fabric for fencing clothing comprises the following steps:

[0084] (1) 10 g of graphene was added to 120 g of ethanol / water solution (ethanol and water were mixed in a volume ratio of 5:1), and then 4 g of KH570 was added dropwise, and the mixture was treated at room temperature and under ultrasonic action for 6 h. The product was centrifuged, washed with alcohol, and dried to obtain double-bond modified graphene;

[0085] (2) 10 g of double bond modified graphene was added to 100 mL of DMF, and then 15.56 g of 2-mercaptoaniline was added and stirred to fully dissolve, and 1 g of methyl benzoylformate was added. The mixture was then irradiated with ultraviolet light at a wavelength of 365 nm and a radiation power of 50 mW / cm 2 The reaction was irradiated for 40 min, and the product was filtered, washed, and dried to obtain aniline graphene;

[0086] (3) 500 g of polycarbonate diol was vacuum dehydrated, mixed evenly with 300 g of isophorone diisocyanate, 10 g of aniline graphene, 20 g of dihydroxyethylglycine and 2000 mL of acetone, nitrogen was continuously introduced, 3 g of dibutyltin dilaurate was added dropwise, the temperature was raised to 75 ° C. and reacted for 4 h. After the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 30 g of 2,2-dihydroxymethylpropionic acid was added. The reaction was continued at 45 ° C. for 2 h, and finally triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0087] (4) 10 g of 250D aramid fiber was washed to remove surface grease, placed in 100 mL of 3 wt% NaOH solution, stirred and reacted at 40° C. for 2 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0088] (5) Preparing aramid fabric using pretreated aramid fiber, immersing the aramid fabric in graphene-modified polyurethane solution, and treating it by dip-rolling process, controlling the coating amount to 25 g / cm 2 , then dried at 80°C for 10 minutes, then heated to 120°C, thermally cured for 2 hours, washed and dried to obtain the modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0089] Comparative Example 2

[0090] A method for preparing a protective fabric for fencing clothing comprises the following steps:

[0091] (1) 10 g of graphene was added to 120 g of ethanol / water solution (ethanol and water were mixed in a volume ratio of 5:1), and then 4 g of KH570 was added dropwise, and the mixture was treated at room temperature and under ultrasonic action for 6 h. The product was centrifuged, washed with alcohol, and dried to obtain double-bond modified graphene;

[0092] (2) 500 g of polycarbonate diol was vacuum dehydrated, and mixed evenly with 300 g of isophorone diisocyanate, 10 g of double-bond modified graphene, 20 g of dihydroxyethylglycine and 2000 mL of acetone, and nitrogen was continuously introduced, and 3 g of dibutyltin dilaurate was added dropwise, and the temperature was raised to 75° C. for reaction for 4 h. After the reaction was completed, the temperature was lowered to room temperature, diluted with acetone, and then 30 g of 2,2-dihydroxymethylpropionic acid was added, and the reaction was continued at 45° C. for 2 h. Finally, triethylamine was added for neutralization to obtain a graphene-modified polyurethane solution;

[0093] (3) 10 g of 250D aramid fiber was washed to remove surface grease, placed in 100 mL of 3 wt% NaOH solution, stirred and reacted at 40° C. for 2 h, and the product was filtered, washed with water, and dried to obtain pretreated aramid fiber;

[0094] (4) Preparing aramid fabrics using pretreated aramid fibers, immersing the aramid fabrics in a graphene-modified polyurethane solution, and treating them by a dip-rolling process, with the coating amount controlled to be 25 g / cm 2 , then dried at 80°C for 10 minutes, then heated to 120°C, thermally cured for 2 hours, washed and dried to obtain the modified aramid fabric, which was cut and sewn to obtain the protective fabric for fencing clothing.

[0095] In Comparative Example 1, due to the presence of amino groups on the surface of aniline graphene, it can participate in the polymerization reaction of polyurethane to a certain extent, and part of the aniline graphene can be bonded to the polyurethane molecular chain to form a cross-linked network structure; the double-bond modified graphene in Comparative Example 2 cannot be chemically bonded to the polyurethane main chain, and it can only be dispersed in the polyurethane solution in the form of filler.

[0096] The protective clothing prepared in Examples 1 to 4 and Comparative Examples 1 to 2 was tested for performance. The breaking strength and breaking elongation of the samples were tested with reference to GB / T 3923.1-2013 "Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break (strip method)"; the puncture strength was measured using an INSTRON 3369 universal strength tester, and the puncture strength of the sample was measured with reference to ASTM F 1342-2005. The size of the sample to be tested was 10 cm × 10 cm, the relative humidity of the test environment was 65%, the test temperature was 20 ° C, and the test speed was 508 mm / min; the air permeability was measured using a YG (B) 461D-Ⅰ digital fabric air permeability meter, and the air permeability of the fabric was tested with reference to GB / T 5453-1997 "Determination of air permeability of textile fabrics", and the sample area was 20 cm 2 , the pressure drop is 100Pa, each sample is tested 10 times, and the results are averaged; refer to EN 1149-1:2006 "Test for electrostatic performance of protective clothing" to test the surface resistance of the fabric, the applied voltage time is 100V, 15s, the temperature is 23±1℃, and the relative humidity is 25±5%; the test results are shown in Table 1.

[0097] Table 1 Test results of protective clothing performance

[0098]

[0099] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a protective fabric for fencing clothing, characterized in that: The method comprises the following steps: preparing aramid fabric with aramid fiber, dipping the aramid fabric in a graphene modified polyurethane solution, washing and drying to obtain the modified aramid fabric, cutting and sewing to obtain the protective fabric for fencing clothing.

2. The preparation method according to claim 1, characterized in that: The method for preparing the graphene-modified polyurethane solution comprises the following steps: (1) adding graphene to an ethanol / water solution, then dropwise adding KH570, ultrasonically treating, centrifuging, washing with alcohol, and drying the product to obtain double-bond modified graphene; (2) adding the double bond modified graphene to DMF, then adding 2-mercaptoaniline and stirring to fully dissolve, adding methyl benzoylformate, reacting under ultraviolet light irradiation, filtering, washing, and drying the product to obtain aniline graphene; (3) dispersing aniline graphene and dihydroxyethylglycine in DMF, ultrasonically treating, adding p-toluenesulfonic acid, heating for reaction, centrifuging the product, and washing with acetone to obtain dihydroxyethyl graphene; (4) The polycarbonate diol is vacuum dehydrated, mixed evenly with isophorone diisocyanate, dihydroxyethylated graphene and acetone, nitrogen is continuously introduced, dibutyltin dilaurate is added dropwise, the temperature is increased for reaction, and after the reaction is completed, the temperature is lowered to room temperature, diluted with acetone, and then 2,2-dihydroxymethylpropionic acid is added to continue the reaction, and finally triethylamine is added for neutralization to obtain a graphene-modified polyurethane solution.

3. The preparation method according to claim 2, characterized in that: In step (1), the ethanol / water solution is obtained by mixing ethanol and water in a volume ratio of 2 to 5:1; the mass ratio of graphene, ethanol / water solution and KH570 is 10:80 to 120:1 to 4; and the ultrasonic treatment conditions are room temperature and ultrasonic treatment for 3 to 6 hours.

4. The preparation method according to claim 2, characterized in that: In step (2), the mass ratio of double bond modified graphene, 2-mercaptoaniline and methyl benzoylformate is 10:8.34-15.56:0.3-1.

5. The preparation method according to claim 2, characterized in that: In step (2), the wavelength of ultraviolet light is 365nm, and the radiation power is 10-50mW / cm 2 , irradiation time 20 to 40 minutes.

6. The preparation method according to claim 2, characterized in that: In step (3), the mass ratio of aniline graphene, dihydroxyethylglycine and p-toluenesulfonic acid is 10:15-30:0.5-3.

7. The preparation method according to claim 2, characterized in that: In step (3), the heating reaction condition is to stir the reaction at 80-110° C. for 10-18 hours.

8. The preparation method according to claim 2, characterized in that: In step (4), the mass ratio of polycarbonate diol, isophorone diisocyanate, dihydroxyethylated graphene, dibutyltin dilaurate, and 2,2-dihydroxymethylpropionic acid is 500:200-300:10:0.5-3:10-30.

9. The preparation method according to claim 2, characterized in that: In step (4), the temperature is raised to 60-75°C for 4-7h; the continued reaction is at 35-45°C for 1-2h.

10. A protective fabric for fencing clothing prepared by the preparation method according to any one of claims 1 to 9.