Printing and dyeing processing method of fabric containing soybean fibers

Through transglutaminase treatment and inactivation treatment, the structural stability of soybean fiber is enhanced, the problem of bleaching of soybean protein fiber fabrics is solved, high breaking strength and whiteness are improved, and its application scope is expanded.

CN118792897APending Publication Date: 2024-10-18JIANGSU GOLDSUN TEXTILE SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410882094.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Due to the presence of textile auxiliaries and pigments, soy protein fiber fabrics naturally appear beige, which requires the use of destructive bleaching agents for bleaching, limiting the richness and application scope of its product types.

Method used

Glutamine transaminase is used to treat soybean fiber. Through enzyme treatment and inactivation treatment steps, the stability of the fiber structure is enhanced to avoid damage to the fiber by bleaching agents. After bleaching, oxidative bleaching or reducing bleaching agents are used to improve the whiteness.

Benefits of technology

It improves the breaking strength and whiteness of soybean fiber fabrics, ensures the effectiveness of the bleaching process, while maintaining other excellent properties of the fiber, and expands its application scope and market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004924856430000071
    Figure BDA0004924856430000071
Patent Text Reader

Abstract

The invention relates to a printing and dyeing processing method of a fabric containing soybean fibers, which comprises the following procedures: desizing, enzyme treatment, bleaching, dyeing, softening and shaping, calendaring and preshrinking, and an enzyme treatment working solution adopted in the enzyme treatment comprises glutamine transaminase with the concentration of 1-3g / L. The fabric containing the soybean fibers is treated through glutamine transaminase after being desized, protein molecules in the soybean fibers can be subjected to a cross-linking reaction under catalysis of the glutamine transaminase, and the cross-linking reaction can enhance the structural stability of the fibers and improve the breaking strength; according to the method, the soybean fibers in the fabric are prevented from being damaged by the subsequent bleaching process, so that the fabric is better bleached, the excellent breaking strength of the fabric is ensured, and the excellent whiteness of the fabric is also ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabric dyeing and finishing, and in particular to a printing and dyeing method for fabric containing soybean fiber. Background Art

[0002] With the continuous advancement of science and technology and the increasing awareness of environmental protection, regenerated fibers, as a sustainable and environmentally friendly material, have received extensive attention and application. Among them, soybean protein fiber, as the only regenerated fiber that has been successfully tested in industrialization by my country, has significant advantages and application prospects.

[0003] The preparation process of soy protein fiber has been carefully designed and optimized. First, protein polymers are extracted from soybean meal, and then a protein spinning solution of a specific concentration is prepared. After maturation, the single fiber tow is gradually spun using wet spinning technology. In order to further stabilize the fiber, it needs to be hydroformylated, followed by cutting, heat setting and curling, and finally various lengths of textile high-grade fibers are produced.

[0004] This fiber not only fully meets environmental protection requirements during the production process and does not cause serious pollution to the environment, but its characteristics also make it widely used in the clothing and home textile industries. Compared with traditional regenerated protein fibers, soybean protein fiber exhibits higher strength and certain antibacterial and health functions. In addition, it has a good affinity with human skin, feels soft and has a soft luster, and has both the hygroscopicity of cotton fiber and the warmth of wool.

[0005] However, despite its many advantages, soy protein fiber still faces a technical challenge: the natural beige color of its fabric. This is caused by the selective absorption of some bands of visible light by impurities such as textile auxiliaries and pigments on the fiber. Therefore, it is necessary to bleach the fabric by oxidative bleaching and / or reductive bleaching in order to completely eliminate this inherent yellow color on the fabric. Unfortunately, bleaching agents are extremely destructive to soy fibers, which not only brings troubles to the dyeing and finishing of soy protein fiber fabrics, but also limits the richness of its product variety. Therefore, this problem has become the main bottleneck restricting the widespread application of soy protein fiber in more fields. Summary of the invention

[0006] The purpose of the present invention is to provide a solution to overcome the above technical difficulties, further expand the application scope of soybean protein fiber, and improve its market competitiveness.

[0007] To achieve the above objectives, this application is implemented through the following technical solutions:

[0008] The present application provides a printing and dyeing method for fabrics containing soybean fiber, comprising the following steps: desizing, enzyme treatment, bleaching, dyeing, softening and shaping, calendering and pre-shrinking. The content of soybean fiber in the fabric is 10% to 100% by weight, and the enzyme treatment working solution used in the enzyme treatment contains glutamine transaminase at a concentration of 1 to 3 g / L.

[0009] As a further improvement of the present application, the temperature of the enzyme treatment is 50-55° C., the time of the enzyme treatment is 40-90 min, and in the enzyme treatment: in terms of weight ratio, the bath ratio of the cloth to the enzyme treatment working solution is 1:5-10.

[0010] As a further improvement of the present application, the enzyme treatment further includes an inactivation treatment step, specifically: adding soda ash to the enzyme treatment working solution, the concentration of the soda ash is 2 to 3 g / L, the temperature of the inactivation treatment is 80 to 90°C, and the time of the inactivation treatment is 20 to 30 minutes.

[0011] As a further improvement of the present application, the bleaching process adopts oxidative bleaching or reductive bleaching, the bleaching agent of the oxidative bleaching is any one of hydrogen peroxide, sodium hypochlorite, and peracetic acid, and the bleaching agent of the reductive bleaching is any one of hydrosulfite, rongalite, thiourea dioxide, and sodium bisulfite.

[0012] As a further improvement of the present application, the dyeing liquid used in the dyeing process includes a reactive dye, and the reactive dye is any one of a vinyl sulfone type reactive dye, a fluoro-s-triazine type reactive dye, and an anthraquinone type reactive dye.

[0013] As a further improvement of the present application, the dyeing solution also includes a dyeing-accelerating salt, and the concentration of the dyeing-accelerating salt is 15 to 20 g / L.

[0014] As a further improvement of the present application, the softening and setting working fluid used in the softening and setting process includes a softener, the concentration of the softener is 20 to 60 g / L, the softening and setting temperature is 160 to 170°C, and the speed of the softening and setting equipment is 40 to 60 m / min.

[0015] As a further improvement of the present application, the process conditions of the calendering process are: pressure of 4 to 5 kg, temperature of 80 to 85° C., and vehicle speed of 20 to 30 m / min.

[0016] As a further improvement of the present application, the process conditions of the pre-shrinking process are: vehicle speed 40-50 m / min, pressure of the pressure roller 6-10 kN, and temperature 100-110°C.

[0017] As a further improvement of the present application, other components in the fabric are one or more of cotton, regenerated cellulose fiber, and synthetic fiber.

[0018] As a further improvement of the present application, a singeing process is further included before the desizing process, or a sanding process is further included after the bleaching process and before the dyeing process.

[0019] As a further improvement of the present application, in the fabric, the proportion of synthetic fibers is less than 30% of the entire fabric and can be subjected to a singeing process. Preferably, the specific process of singeing is: the burner temperature is 1100-1200°C and the vehicle speed is 100-110m / min.

[0020] As a further improvement of the present application, the fabric containing soybean fiber may have a plain, twill or satin weave structure, and the warp and weft yarn counts are 21s to 100s.

[0021] The beneficial effect of the present application is that the fabric containing soybean fiber of the present application is first treated with glutamine transaminase after desizing. Under the catalysis of glutamine transaminase, a cross-linking reaction can occur between the protein molecules in the soybean fiber. This cross-linking reaction can enhance the structural stability of the fiber, improve the breaking strength, avoid the subsequent bleaching process from damaging the soybean fiber in the fabric, and thus achieve better bleaching, which not only ensures that the fabric has excellent breaking strength, but also ensures that the fabric has excellent whiteness. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0023] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with specific implementation methods.

[0024] Example 1

[0025] This embodiment provides a printing and dyeing method for fabrics containing soybean fiber.

[0026] The fabric specifications are: 105" / (Tencel / soy fiber / combed cotton 50 / 30 / 20) 60S tight*(Tencel / soy fiber / combed cotton 50 / 30 / 20) 60S tight / 200*100 4 / 1 satin. Specifically: the above fabric is a 60-spindle fabric with a width of 105 inches, a blend of 50% Tencel, 30% soybean fiber and 20% combed cotton, a warp and weft density of 200*100, and a 4 / 1 satin weave.

[0027] The steps of fabric printing and dyeing are as follows: the fabric is subjected to the steps of turning the seam ends, singeing, desizing, enzyme treatment, bleaching, dyeing, softening and shaping, calendering and pre-shrinking in sequence to prepare the fabric containing soybean fiber after printing and dyeing, wherein:

[0028] Turning and sewing the cloth: It is the process of turning the cloth over, arranging it, and placing it on a cloth pile board or a clean cloth cart, and then connecting the turned cloth box by box with a sewing machine.

[0029] In the singeing process: the burner temperature is 1000-1100℃, the machine speed is 100-110m / min, and a combination of four burners, two positive and two negative, is adopted.

[0030] In the desizing process: biological enzyme desizing is adopted. After singeing, the fabric is directly immersed in the desizing working solution containing biological enzyme. The desizing working solution contains biological enzyme with a concentration of 5g / L and a penetrant with a concentration of 2g / L. After extinguishing the fire, it is piled at room temperature for 12h to 16h.

[0031] In the enzyme treatment process: the enzyme treatment is carried out in a dyeing machine, and the treatment conditions are: the enzyme treatment working solution contains 3g / L glutamine transaminase, the enzyme treatment temperature is 50°C, the enzyme treatment time is 40min, and in the enzyme treatment: the bath ratio of the cloth to the enzyme treatment working solution is 1:5 by weight. After the enzyme treatment, the step of inactivation treatment is also included, specifically: adding soda ash to the enzyme treatment working solution, the concentration of soda ash is 2g / L, the inactivation treatment temperature is 80°C, and the inactivation treatment time is 30min.

[0032] In the bleaching process: the bleaching agent used in the bleaching process includes hydrogen peroxide and hydrogen peroxide stabilizer, the concentration of hydrogen peroxide is 2.5g / L, the concentration of hydrogen peroxide stabilizer is 2g / L, the bleaching temperature is 95°C, the bleaching time is 1.5h, and the cloth is dried.

[0033] In the dyeing process: the dyeing liquid used in the dyeing process contains anthraquinone type active dye, leveling agent and bath treasure with a concentration of 1g / L. The dyeing liquid is used to dye the cloth after the bleaching process. After the color fixing water washing, the cloth is taken out and dried.

[0034] In the softening and setting process: the softening and setting working fluid used in the softening and setting process includes a softener, the concentration of the softener is 40g / L, the softening and setting temperature is 165°C, the speed of the softening and setting equipment is about 60m / min, and the cloth can be dried.

[0035] Calendering process: pressure is 4-5kg, temperature is 80-85℃, speed is 20-30m / min.

[0036] Pre-shrinking process: machine speed 40-50m / min, pressure of pressure roller 6-10kN, temperature 100-110℃.

[0037] Example 2

[0038] This embodiment provides a printing and dyeing method for fabrics containing soybean fiber.

[0039] The fabric specifications are: 105" / (Tencel / soybean fiber 50 / 50) 40S Saijin*(Tencel / soybean fiber 50 / 50) 40S Saijin / 144*80 4 / 1 satin. Specifically: the above fabric is a 40-spindle fabric with a width of 105 inches, a blend of 50% Tencel and 50% soybean fiber, a warp and weft density of 144*80, and a 40-spindle fabric with a 4 / 1 satin weave.

[0040] The steps of fabric printing and dyeing are as follows: the fabric is subjected to the steps of turning the seam ends, desizing, enzyme treatment, bleaching, dyeing, softening and shaping, calendering and pre-shrinking in sequence to prepare the fabric containing soybean fiber after printing and dyeing, wherein:

[0041] Turning and sewing the cloth: It is the process of turning the cloth over, arranging it, and placing it on a cloth pile board or a clean cloth cart, and then connecting the turned cloth box by box with a sewing machine.

[0042] In the desizing process: biological enzyme desizing is adopted. After the fabric is singed, it is directly inserted into the desizing working solution containing biological enzymes. The desizing working solution contains biological enzymes with a concentration of 6g / L and a penetrant with a concentration of 4g / L. After extinguishing the fire, it is piled at room temperature for 16 hours.

[0043] In the enzyme treatment process: the enzyme treatment is carried out in a dyeing machine, and the treatment conditions are: the enzyme treatment working solution contains glutamine aminotransferase with a concentration of 2g / L, the enzyme treatment temperature is 55°C, and the enzyme treatment time is 60min. In the enzyme treatment: the bath ratio of the cloth to the enzyme treatment working solution is 1:8 by weight. After the enzyme treatment, the step of inactivation treatment is also included, specifically: adding soda ash to the enzyme treatment working solution, the concentration of soda ash is 3g / L, the inactivation treatment temperature is 90°C, and the inactivation treatment time is 25min.

[0044] In the bleaching process: the bleaching agent used in the bleaching process includes hydrogen peroxide and hydrogen peroxide stabilizer, the concentration of hydrogen peroxide is 1.5g / L, the concentration of hydrogen peroxide stabilizer is 1g / L, the bleaching temperature is 95°C, the bleaching time is 4h, and the cloth is dried.

[0045] In the dyeing process: the dyeing liquid used in the dyeing process contains monofluorotriazine type active dye, leveling agent and bath treasure with a concentration of 1g / L. The dyeing liquid is used to dye the cloth after the bleaching process. After the color fixing water washing, the cloth is taken out and dried.

[0046] In the softening and setting process: the softening and setting working fluid used in the softening and setting process includes a softener, the concentration of the softener is 50g / L, the softening and setting temperature is 170°C, the speed of the softening and setting equipment is about 50m / min, and the cloth can be dried.

[0047] Calendering process: pressure is 4-5kg, temperature is 80-85℃, speed is 20-30m / min.

[0048] Pre-shrinking process: machine speed 40-50m / min, pressure of pressure roller 6-10kN, temperature 100-110℃.

[0049] Example 3

[0050] The difference between this embodiment and embodiment 1 is that in the enzyme treatment process: the enzyme treatment is carried out in a dye roller, the treatment conditions are: the enzyme treatment working solution contains glutamine transaminase with a concentration of 2 g / L, the enzyme treatment temperature is 52°C, the enzyme treatment time is 60 min, and in the enzyme treatment: the bath ratio of the cloth to the enzyme treatment working solution is 1:8 by weight.

[0051] Example 4

[0052] The difference between this embodiment and embodiment 1 is that in the enzyme treatment process: the enzyme treatment is carried out in a dye roller, the treatment conditions are: the enzyme treatment working solution contains glutamine transaminase with a concentration of 1 g / L, the enzyme treatment temperature is 55°C, the enzyme treatment time is 90 minutes, and in the enzyme treatment: the bath ratio of the cloth to the enzyme treatment working solution is 1:10 by weight.

[0053] Comparative Example 1

[0054] This comparative example is different from Example 1 in that it does not include an enzyme treatment step.

[0055] Comparative Example 2

[0056] This comparative example is different from Example 1 in that it does not include an inactivation treatment step after the enzyme treatment.

[0057] Comparative Example 3

[0058] The difference between this embodiment and embodiment 1 is that in the enzyme treatment process: the enzyme treatment is carried out in a dye roller, the treatment conditions are: the enzyme treatment working solution contains 4 g / L glutamine transaminase at a concentration of 4 g / L, the enzyme treatment temperature is 55°C, the enzyme treatment time is 90 min, and in the enzyme treatment: in terms of weight ratio, the bath ratio of the cloth to the enzyme treatment working solution is 1:5.

[0059] According to the standard, the breaking strength of the semi-finished products of Examples 1 to 4 and Comparative Examples 1 to 3, as well as the whiteness and breaking strength of the finished products were tested and evaluated, and the results are shown in Table 1, wherein the semi-finished product refers to the cloth after bleaching, and the finished product refers to the cloth after pre-shrinkage, wherein J represents the radial parameter of the cloth, and W represents the weft parameter of the cloth.

[0060] Table 1

[0061]

[0062] According to the requirements of the existing standard GB 18401-2010 "National Textile Basic Safety Technical Code", the weft tensile breaking strength of the fabric ≥250N is the national first-class product, the weft tensile breaking strength ≥220N is a qualified product, and the weft tensile breaking strength <220N is an unqualified product.

[0063] According to the above-mentioned test results of the breaking strength, elongation at break and whiteness of the cloth after printing and dyeing of Examples 1-4 and Comparative Examples 1-3, the cloth after bleaching has excellent whiteness. However, according to the comparison between Comparative Example 1 and Examples 1-4, the breaking strength of the semi-finished product of the cloth not treated with enzyme after bleaching and the breaking strength of the finished product after pre-shrinkage are much lower than the breaking strength of the cloth treated with enzyme. According to the comparison between Comparative Example 2 and Examples 1-4, the breaking elongation of the semi-finished product of the cloth not treated with inactivation after enzyme treatment is reduced, which affects the breaking strength of the final finished product, causing the breaking strength of the finished product to be reduced. According to the comparison between Comparative Example 3 and Examples 1-4, the concentration of the enzyme in the enzyme treatment solution is too high, which will also cause the breaking elongation of the semi-finished product to be reduced, thereby lowering the breaking strength of the final finished product.

[0064] Fabrics containing soybean fiber treated with glutamine transaminase (TGase) have better whiteness and strength indicators.

[0065] Although the tensile elongation at break is not included in the national standard for textile product quality assessment, it reflects the softness and elasticity of the fabric to a certain extent. Textiles with good softness and elasticity are more popular in the market, and the greater the elongation, the softer the fabric, the better the elasticity, and the easier the fabric is to deform; if the elongation is too small, the fabric feels poor and has less elasticity. According to multiple current tests and studies, the best range of the tensile elongation at break of fabric is 10-20%.

[0066] In addition, the concentration, treatment time and bath ratio of TGase are all very important factors affecting the tensile fracture performance index of fabrics. The higher the concentration, the higher the bath ratio, the shorter the treatment time and the higher the efficiency. However, if the concentration is too high, the cross-linking reaction of protein molecules will be very intense, affecting the ductility of the fabric. After the enzyme treatment, it is necessary to inactivate the enzyme, otherwise the cross-linking reaction will still occur, and eventually the strength will be reduced due to excessive cross-linking.

[0067] The fabric containing soybean fiber of the present application is first treated with glutamine aminotransferase after desizing. The soybean fiber contains protein molecules and polyvinyl alcohol, which are incompatible. The soybean protein is usually dispersed in the polyvinyl alcohol component of the continuous phase in a lumpy and discontinuous state.

[0068] Under the catalysis of glutamine transaminase, cross-linking reactions can occur between protein molecules in soybean fiber. Specifically, TGase can catalyze the amido transfer reaction between the γ-amide group of glutamine residues in proteins and the ε-amino group of lysine to form a heterotypic peptide bond of ε-(γ-glutamine)-lysine. This cross-linking reaction can enhance the structural stability of the fiber and improve the breaking strength. However, glutamine transaminase cannot directly act on polyvinyl alcohol molecules for cross-linking reactions, but it can catalyze the cross-linking within the soybean protein molecules through enzymes, thereby affecting the arrangement and interaction of polyvinyl alcohol molecules, thereby enhancing the structural stability of the fiber and improving the breaking strength.

[0069] In addition, the treatment process of glutamine transaminase does not involve changes in the color of the fiber. Under the catalysis of glutamine transaminase, the breaking strength of the fabric is improved and its strength is stabilized within a preset range, ensuring that the fabric also has excellent ductility. The excellent strength of the fabric can ensure that the fabric is not damaged in the subsequent bleaching process, so that the fabric can be bleached well, thereby ensuring excellent whiteness without affecting other properties of the fabric.

[0070] Although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0071] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present application. They are not intended to limit the scope of protection of the present application. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present application should be included in the scope of protection of the present application.

Claims

1. A printing and dyeing method for fabrics containing soybean fiber, It is characterized in that The process comprises the following steps: desizing, enzyme treatment, bleaching, dyeing, softening and shaping, calendering and pre-shrinking. The content of soybean fiber in the fabric is 10% to 100% by weight, and the enzyme treatment working solution used in the enzyme treatment contains 1 to 3 g / L glutamine aminotransferase.

2. The printing and dyeing method of the fabric containing soybean fiber according to claim 1, It is characterized in that The temperature of the enzyme treatment is 50-55° C., the time of the enzyme treatment is 40-90 min, and in the enzyme treatment: in terms of weight ratio, the bath ratio of the cloth to the enzyme treatment working solution is 1:5-10.

3. The printing and dyeing method of the fabric containing soybean fiber according to claim 2, It is characterized in that The enzyme treatment further includes an inactivation treatment step, which is specifically: adding soda ash to the enzyme treatment working solution, the concentration of the soda ash is 2-3 g / L, the temperature of the inactivation treatment is 80-90° C., and the time of the inactivation treatment is 20-30 minutes.

4. The printing and dyeing method of the fabric containing soybean fiber according to claim 1, It is characterized in that The bleaching process adopts oxidation bleaching or reduction bleaching, the bleaching agent of the oxidation bleaching is any one of hydrogen peroxide, sodium hypochlorite and peracetic acid, and the bleaching agent of the reduction bleaching is any one of hydrosulfite, Rongalite, thiourea dioxide and sodium bisulfite.

5. The printing and dyeing method of the fabric containing soybean fiber according to claim 1, It is characterized in that The dyeing liquid used in the dyeing process includes a reactive dye, and the reactive dye is any one of a vinyl sulfone type reactive dye, a fluoro-s-triazine type reactive dye, and an anthraquinone type reactive dye.

6. The printing and dyeing method of the fabric containing soybean fiber according to claim 5, It is characterized in that The dyeing solution also includes a dyeing-accelerating salt, and the concentration of the dyeing-accelerating salt is 15-20 g / L.

7. The printing and dyeing method of the fabric containing soybean fiber according to claim 1, It is characterized in that The softening and setting working fluid used in the softening and setting process includes a softener, the concentration of the softener is 20-60 g / L, the softening and setting temperature is 160-170° C., and the speed of the softening and setting equipment is 40-60 m / min.

8. The printing and dyeing method of the fabric containing soybean fiber according to claim 1, It is characterized in that The process conditions of the calendering process are: pressure of 4-5kg, temperature of 80-85°C, and vehicle speed of 20-30m / min.

9. The printing and dyeing method of fabric containing soybean fiber according to claim 1, It is characterized in that The process conditions of the pre-shrinking process are: vehicle speed 40-50 m / min, pressure of the pressure roller 6-10 kN, and temperature 100-110°C.

10. The printing and dyeing method of fabric containing soybean fiber according to claim 1, It is characterized in that Other components in the fabric are one or more of cotton, regenerated cellulose fiber and synthetic fiber.