Mixed rubber material combined powder, recyclable compressed bonded magnet and preparation method of recyclable compressed bonded magnet
Through the ratio of rubber compound powder and thermoplastic resin with different particle sizes, the problem of deformation of rare earth bonded magnets during use of thermoplastic resin is solved, high-temperature stability and recyclability are improved, and costs and processing waste are reduced. .
Patent Information
- Application Number
- CN202410772841.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
AI Technical Summary
When rare earth bonded magnets use thermoplastic resin as a binder, due to their low thermal deformation temperature and poor high-temperature stability, they are prone to deformation during the compression molding process, resulting in non-compliance with product specifications and increased processing costs.
Using rubber compound powders of different particle sizes, the fit and mechanical strength of the magnetic powders are improved through the different particle size combinations of magnetic powders and coating with thermoplastic resin to ensure that no deformation occurs during the heat treatment process.
It achieves excellent recyclability and shape stability of rare earth bonded magnets, reduces the cost of recycled magnets, reduces processing waste, and meets high temperature stability and shape requirements.
Smart Images

Figure BDA0004895641210000181 
Figure BDA0004895641210000211 
Figure BDA0004895641210000231
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnets, and in particular to a mixed rubber composite powder, a recyclable compressed bonded magnet and a preparation method thereof. Background Art
[0002] Rare earth bonded magnets have the characteristics of high dimensional accuracy, good magnetic property consistency, large shape freedom, high resistivity and low eddy current loss, and are therefore widely used in the fields of computers, consumer electronics, energy-saving home appliances, and the automotive industry. The preparation of rare earth bonded magnets is generally made by compression molding, injection molding, or extrusion molding, and the mixture of rare earth magnetic powder and binder is pressed and molded into the required shape. Among them, the compression molding process usually uses thermosetting resins (such as epoxy resins) as binders. The bonded magnets prepared by this process have the advantages of high magnetic powder filling rate, high mechanical strength, good high temperature stability, and high magnetic properties.
[0003] In recent years, due to the scarcity of rare earth resources, the demand for the recycling and reuse of rare earth bonded magnets has become increasingly high. However, thermosetting resins are cured and cross-linked once, and it is difficult to recycle and reuse them after cross-linking and curing. If thermoplastic resins are used instead of thermosetting resins as binders to prepare compressed bonded magnets, the demand for the recycling and reuse of bonded magnets can be met. However, due to the low thermal deformation temperature and poor high temperature stability of thermoplastic resins, magnet deformation is prone to occur during the compression molding process.
[0004] Therefore, it is necessary to develop a new method and product for preparing a compressed bonded magnet using a thermoplastic resin that can prevent the magnet from deforming. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a mixed rubber combination powder, a recyclable compressed bonded magnet and a preparation method thereof. The combination ratio of magnetic powders with different particle sizes is used to enhance the fit between the magnetic powders, and magnetic powders of different particle sizes are mixed with thermoplastic resins in corresponding proportions to prepare mixed rubber combination powders with different particle sizes. The mixed rubber combination powder is then used for compression molding and heat treatment. The obtained magnet not only has excellent recyclability, but also will not deform during the heat treatment process.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In the first aspect, the present invention provides a mixed rubber combination powder for recyclable compressed bonded magnets, the mixed rubber combination powder includes mixed rubbers with different particle sizes, the mixed rubbers include magnetic powder and a thermoplastic resin coated on the surface of the magnetic powder; the particle sizes of the magnetic powders in the mixed rubbers with different particle sizes are different; when the particle size of the magnetic powder in any mixed rubber is larger than the particle size of the magnetic powder in any other mixed rubber, the mass ratio of the thermoplastic resin in the mixed rubber to the magnetic powder is smaller than the mass ratio of the thermoplastic resin to the magnetic powder in any other mixed rubber.
[0008] It is worth noting that the conventional process for preparing bonded magnets by compression molding is to use thermosetting resins such as epoxy resins as binders. Based on the background of recycling and reuse, although the bonded magnets prepared by thermosetting binders have excellent mechanical properties and high temperature resistance, the thermosetting resin is difficult to recycle after cross-linking and curing once formed. Therefore, it is necessary to consider using thermoplastic resins instead of thermosetting resins as binders to prepare bonded magnets by compression molding. However, the technical problems that need to be further solved when using thermoplastic resins as binders are: due to the low thermal deformation temperature and poor high-temperature stability of thermoplastic resins, magnet deformation is easily generated during the compression molding process of preparing bonded magnets, and the magnet deformation problem makes it difficult to meet product specifications or requires subsequent machining to meet product specifications, which in turn causes a series of problems such as increased processing costs and the generation of waste materials.
[0009] Based on the above difficulties, the inventors creatively use mixed rubber materials with different particle sizes for combination, and the particle sizes of the magnetic powder inside the first mixed rubber material, the second mixed rubber material, the third mixed rubber material, the fourth mixed rubber material and the fifth mixed rubber material are different, that is, mixed rubber materials with different particle sizes and magnetic powders with different particle sizes inside the mixed rubber materials are used in combination. Based on this, the present application is to coat a specific amount of thermoplastic resin on the surface of magnetic powders with different particle sizes, so that the amount of thermoplastic resin on the surface of magnetic powders with different particle sizes is less different, so that a large amount of aggregated thermoplastic resin will not be deformed during the subsequent heat treatment process.
[0010] Based on the above, the core invention of the present invention lies in the following three key points:
[0011] 1. The magnetic powder is ground by ball milling or air flow milling to repair irregular shapes, reduce non-spherical coefficients, and reduce the surface roughness of the magnetic powder, thereby increasing the tap density and packing density of subsequent loading and reducing the deformation space of subsequent processes;
[0012] 2. Use mixed rubber materials of different particle sizes to combine, use fine powder to fill gaps and fine powder to adhere to the surface of irregular large particles. The combination of particle sizes can increase the tap density and packing density of the mixed rubber material and reduce the deformable space in the subsequent process;
[0013] 3. Magnetic powders of different particle sizes are respectively mixed with thermoplastic resins in corresponding proportions to prepare mixed rubber materials. The usual process is to first mix the magnetic powders of different particle sizes uniformly and then mix them with the thermoplastic resin. However, due to the different specific surface areas of coarse powder and fine powder, the proportion of thermoplastic resin on the surface of fine powder is too high, and the proportion of thermoplastic resin on the surface of coarse powder is relatively small. The uneven distribution of thermoplastic resin will cause deformation of the compressed magnet during heat treatment. The present invention uses magnetic powders of different particle sizes in mixed rubber materials of different particle sizes and sets thermoplastic resins in corresponding proportions, that is, magnetic powders of different particle sizes are first mixed with thermoplastic resins separately, so that the thermoplastic resins are evenly distributed on the surfaces of magnetic powders with different specific surface areas. The thermoplastic resins that soften and flow during the subsequent compression and heat treatment process are separated by the magnetic powders that do not melt and flow, so that more thermoplastic resins are prevented from gathering at local positions of the magnet, thereby maintaining the shape of the entire magnet unchanged.
[0014] Preferably, the mixed rubber includes a first mixed rubber, a second mixed rubber, a third mixed rubber, a fourth mixed rubber and a fifth mixed rubber; wherein the particle size and mass distribution of the magnetic powder in the first mixed rubber, the second mixed rubber, the third mixed rubber, the fourth mixed rubber and the fifth mixed rubber are:
[0015] The magnetic powder particle size in the first mixed rubber material is less than 40 μm 10-18 wt%;
[0016] The magnetic powder particle size in the second rubber mixture is 40-75 μm, 30-40 wt%;
[0017] The magnetic powder particle size in the third mixed rubber material is 75-100 μm 30-40 wt%;
[0018] The magnetic powder particle size in the fourth mixed rubber material is 100-150 μm and 12-20 wt%;
[0019] The particle size of the magnetic powder in the fifth mixed rubber is >150 μm 0-1wt%.
[0020] The above mass distribution is the mass fraction of magnetic powder with this particle size to all magnetic powder.
[0021] There are many factors that affect the loose density of powders, such as powder particle shape, size, surface roughness and particle size distribution. Generally speaking, the loose density of powders decreases with the decrease in particle size, the increase in particle non-sphericity coefficient and the increase in surface roughness. The appropriate ratio of different particle sizes is an effective method to improve the loose density. The mass distribution of different particle sizes of the magnetic powder of the present invention preferably adopts the above requirements, and the fine powder fills the gaps, and the fine powder adheres to the surface of the coarse powder to spheroidize the irregular coarse powder, reduce the non-sphericity coefficient and reduce the surface roughness. Moreover, in the present invention, powders finer than coarse powders can be called fine powders, that is, the surface of the coarse powder can be adhered with slightly fine, medium fine and very fine powders, which can be more conducive to spheroidization.
[0022] The particle size of the magnetic powder in the first mixed rubber is less than 40 μm, and the magnetic powder in the first mixed rubber accounts for 10 to 18 wt % of the magnetic powder in all the mixed rubbers, for example, it can be 10 wt %, 11 wt %, 12 wt %, 13 wt %, 14 wt %, 15 wt %, 16 wt %, 17 wt %, 18 wt % or 18 wt %, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0023] The particle size of the magnetic powder in the second mixed rubber is 40-75 μm, and the magnetic powder in the second mixed rubber accounts for 30-40 wt% of the magnetic powder in all the mixed rubbers, for example, it can be 30 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt% or 40 wt%, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0024] The particle size of the magnetic powder in the third mixed rubber is 75-100 μm, and the magnetic powder in the third mixed rubber accounts for 30-40 wt% of the magnetic powder in all mixed rubbers, for example, it can be 30 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt% or 40 wt%, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0025] The particle size of the magnetic powder in the fourth mixed rubber is 100-150 μm, and the magnetic powder in the fourth mixed rubber accounts for 12-20 wt% of the magnetic powder in all mixed rubbers, for example, it can be 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt% or 20 wt%, etc., but is not limited to the listed values, and other values not listed within the range are also applicable.
[0026] The particle size of the magnetic powder in the fifth mixed rubber is >150μm, and the magnetic powder in the fifth mixed rubber accounts for 0-1wt% of the magnetic powder in all mixed rubbers, for example, it can be 0wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0027] Preferably, the material of the magnetic powder includes any one of NdFeB magnetic powder, SmFeN magnetic powder, NdFeN magnetic powder or SmCo magnetic powder, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of NdFeB magnetic powder and SmFeN magnetic powder, a combination of NdFeN magnetic powder and SmFeN magnetic powder, a combination of NdFeB magnetic powder and NdFeN magnetic powder, and a combination of SmCo magnetic powder and SmFeN magnetic powder.
[0028] Preferably, the bulk density of the magnetic powder is 3.0-3.3 g / cm 3 , for example, it can be 3.0 g / cm 3 、3.05g / cm 3 、3.10g / cm 3 、3.15g / cm 3 、3.2g / cm 3 、3.24g / cm 3 、3.27g / cm 3 or 3.3 g / cm 3 The above values are not limited to the above values, and other values not listed in the above values are also applicable.
[0029] Preferably, the tap density of the magnetic powder is 3.5 to 3.9 g / cm 3 , for example, it can be 3.5g / cm 3 、3.52g / cm 3 、3.55g / cm 3 、3.58g / cm 3 、3.60g / cm 3 、3.62g / cm 3 、3.65g / cm 3 、3.7g / cm 3 、3.75g / cm 3 、3.79g / cm 3 、3.84g / cm 3 、3.88g / cm 3 or 3.9g / cm 3 The above values are not limited to the above values, and other values not listed in the above values are also applicable.
[0030] Preferably, the mass fraction of thermoplastic resin in the mixed rubber composite powder to magnetic powder is a, wherein a ranges from 1.8 to 3.0wt%, wherein a ranges from 1.8 to 3.0wt%, for example, it can be 1.8wt%, 2wt%, 2.1wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.8wt%, 2.9wt% or 3.0wt%, etc., but is not limited to the listed values, and other values not listed within the range are equally applicable.
[0031] Preferably, in the first rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.6a to 2.2a, for example, 1.6a, 1.7a, 1.8a, 1.9a, 2a, 2.1a or 2.2a, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0032] Preferably, in the second rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.1a-1.5a, for example, 1.1a, 1.2a, 1.3a, 1.4a or 1.5a, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0033] Preferably, in the third rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.5a-0.9a, for example, 0.5a, 0.6a, 0.7a, 0.8a or 0.9a, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0034] Preferably, in the fourth rubber mixture, the mass ratio of thermoplastic resin to magnetic powder is 0.2a-0.5a, for example, it can be 0.2a, 0.25a, 0.3a, 0.35a, 0.4a, 0.45a or 0.5a, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0035] Preferably, in the fifth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.1a-0.3a, for example, 0.1a, 0.15a, 0.2a, 0.25a or 0.3a, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0036] Preferably, the particle size of the first mixed rubber is less than 75 μm, for example, it can be 45 μm, 49 μm, 52 μm, 55 μm, 59 μm, 62 μm, 65 μm, 69 μm, 72 μm or 75 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0037] Preferably, the particle size of the second rubber mixture is 75-100 μm, for example, it can be 75 μm, 76 μm, 78 μm, 80 μm, 82 μm, 85 μm, 90 μm, 95 μm or 100 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0038] Preferably, the particle size of the third mixed rubber is 100-150 μm, for example, it can be 100 μm, 110 μm, 115 μm, 120 μm, 125 μm, 130 μm, 135 μm, 140 μm, 145 μm or 150 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0039] Preferably, the particle size of the fourth rubber mixture is 150-250 μm, for example, it can be 150 μm, 155 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm or 250 μm, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0040] Preferably, the particle size of the fifth mixed rubber is 150-250 μm, for example, it can be 150 μm, 155 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm or 250 μm, etc., but it is not limited to the listed values, and other unlisted values within this range are also applicable. It is worth noting that the recyclable compressed bonded magnets targeted by the present invention are generally thin-walled products, such as 1 mm, etc., so it is necessary to control the size of the fourth mixed rubber and the fifth mixed rubber to avoid the situation where it is difficult to fill into the mold cavity. Moreover, the particle size range of the fourth mixed rubber and the fifth mixed rubber can be consistent, and both provide a larger particle basis to facilitate the first mixed rubber, the second mixed rubber and the third mixed rubber to fill into the pores.
[0041] Preferably, the bulk density of the mixed rubber is 3.2-3.5 g / cm 3 , for example, it can be 3.2 g / cm 3 、3.24g / cm 3 、3.27g / cm 3 、3.3g / cm 3 、3.34g / cm 3 3.37g / cm 3 、3.4g / cm 3 、3.44g / cm 3 、3.47g / cm 3 or 3.5g / cm 3 The above values are not limited to the above values, and other values not listed in the above values are also applicable.
[0042] The present invention adopts mixed rubber materials with different particle sizes to increase the bulk density of the conventional process to 3.0g / cm 3 Increase to 3.2~3.5g / cm 3 between.
[0043] Preferably, the tap density of the mixed rubber is 3.7-4.1 g / cm 3 , for example, it can be 3.7 g / cm 3 、3.75g / cm 3 、3.79g / cm 3 、3.84g / cm 3、3.88g / cm 3 、3.93g / cm 3 、3.97g / cm 3 4.02g / cm 3 4.06g / cm 3 or 4.1 g / cm 3 The above values are not limited to the above values, and other values not listed in the above values are also applicable.
[0044] The present invention adopts mixed rubber materials with different particle sizes to increase the tap density of the conventional process to 3.4g / cm 3 Increase to 3.7~4.1g / cm 3 The fit between the magnetic powders is enhanced, the mechanical strength before heat treatment is improved, and the deformation of the magnet caused by the melting of the thermoplastic resin during heat treatment is avoided.
[0045] Preferably, the thermoplastic resin comprises any one of nylon, polyphenylene sulfide, polyimide or polypropylene, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of nylon and polyphenylene sulfide, a combination of polyimide and polyphenylene sulfide, and a combination of nylon and polyimide.
[0046] In a second aspect, the present invention provides a recyclable compressed bonded magnet, which includes the mixed rubber combination powder for recyclable compressed bonded magnets described in the first aspect; the recyclable compressed bonded magnet includes magnetic powder and thermoplastic resin, and the mass fraction of the thermoplastic resin in the magnetic powder is 1.8 to 3.0 wt%.
[0047] Among them, 1.8~3.0wt% can be, for example, 1.8wt%, 2wt%, 2.1wt%, 2.2wt%, 2.4wt%, 2.5wt%, 2.6wt%, 2.8wt%, 2.9wt% or 3.0wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0048] Preferably, the material of the magnetic powder is any one of NdFeB magnetic powder, SmFeN magnetic powder, NdFeN magnetic powder or SmCo magnetic powder, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of NdFeB magnetic powder and SmFeN magnetic powder, a combination of NdFeN magnetic powder and NdFeN magnetic powder, a combination of NdFeN magnetic powder and SmFeN magnetic powder, and a combination of SmCo magnetic powder and SmFeN magnetic powder.
[0049] Preferably, the thermoplastic resin comprises any one of nylon, polyphenylene sulfide, polyimide or polypropylene, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of nylon and polyphenylene sulfide, a combination of polyimide and polyphenylene sulfide, and a combination of nylon and polyimide.
[0050] Preferably, the recyclable compressed bonded magnet also includes a lubricant accounting for 0.1 to 0.5 wt% of the total mass of the magnetic powder and the thermoplastic resin, for example, it can be 0.1 wt%, 0.12 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt% or 0.5 wt%, etc.
[0051] Preferably, the lubricant comprises a stearate, preferably zinc stearate.
[0052] Preferably, the roundness of the recyclable compressed bonded magnet is ≤0.06 mm, for example, it may be 0.06 mm, 0.05 mm, 0.04 mm, 0.03 mm, 0.02 mm, 0.01 mm or 0 mm.
[0053] Preferably, the coaxiality of the recyclable compressed bonded magnet is ≤0.08 mm, for example, it may be 0.08 mm, 0.07 mm, 0.06 mm, 0.05 mm, 0.04 mm, 0.03 mm or 0.02 mm.
[0054] Preferably, the recyclable compressed bonded magnet The crushing force of the ring is ≥100N, for example, it can be 100N, 110N, 115N, 120N, 125N, 129N or 130N.
[0055] It is worth noting that the above data on coaxiality, roundness and crushing force are based on the data support range of the ring shape as an example, but there is no special limitation on the shape of the bonded magnet in the present invention, and different shapes can be adopted according to actual needs.
[0056] Preferably, the proportion of recycled powder added to the recyclable compressed bonded magnet each time is ≤30wt%, for example, it can be 30wt%, 29wt%, 28wt%, 27wt%, 26wt%, 25wt%, 20wt%, 19wt% or 18wt%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0057] Preferably, compared with a brand new recyclable compressed bonded magnet, the residual magnetism of the recyclable compressed bonded magnet after N times of reuse is reduced by <2%, and the crushing force of the magnetic ring is reduced by <1%, where N≥1, for example, it can be 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, etc.
[0058] The recyclable compressed bonded magnet provided by the present invention has excellent recycling performance and broad application prospects.
[0059] Among them, the residual magnetism after N times of reuse is reduced by <2%, for example, it can be 1.9%, 1.8%, 1.7%, 1.6%, 1.5%, 1.4%, 1.3%, 1.2% or 1.0%, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0060] The crushing force of the magnetic ring is reduced by <1%, for example, it can be 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4% or 0.3%, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0061] In a third aspect, the present invention provides a method for preparing the recyclable compressed bonded magnet described in the second aspect, wherein the preparation method adopts the mixed rubber combination powder for the recyclable compressed bonded magnet described in the first aspect.
[0062] The preparation method of the recyclable compressed bonded magnet provided by the present invention adopts the mixed rubber composite powder described in the first aspect, and can adopt conventional compression molding and heat treatment processes, which is simple to operate and has broad application prospects.
[0063] Preferably, the preparation method comprises:
[0064] (1) Magnetic powders of different particle sizes are mixed with thermoplastic resins and crushed separately to obtain mixed rubber composite powders composed of mixed rubbers of different particle sizes;
[0065] (2) mixing a lubricant and the mixed rubber powder of step (1), filling the mixture into a mold, and performing compression molding and demolding in sequence to obtain a bonded magnet blank;
[0066] (3) The bonded magnet formed blank in step (2) is heat treated to obtain a recyclable compressed bonded magnet.
[0067] Preferably, the crushing in step (1) is carried out using a vibrating crushing and screening machine.
[0068] Preferably, before the separate mixing, the preparation method further comprises: grinding the magnetic powder by ball milling or air jet milling.
[0069] The grinding method of the present invention can round the sharp corners of the magnetic powder and obtain the magnetic powder with the target particle size.
[0070] Preferably, the ball-to-material ratio of the ball mill is 0.5:1 to 3:1, for example, it can be 0.5:1, 0.8:1, 1.1:1, 1.4:1, 1.7:1, 1.9:1, 2.2:1, 2.5:1, 2.8:1 or 3:1, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0071] Preferably, the ball milling time is 20 to 60 min, for example, 20 min, 25 min, 29 min, 34 min, 38 min, 43 min, 47 min, 52 min, 56 min or 60 min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0072] Preferably, the diameter of the grinding balls in the ball mill is 5 to 12 mm, for example, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm or 12 mm, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0073] Preferably, the rotation speed of the ball mill is 300-800 r / min, for example, it can be 300 r / min, 356 r / min, 412 r / min, 467 r / min, 523 r / min, 578 r / min, 634 r / min, 689 r / min, 745 r / min or 800 r / min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0074] Preferably, the compression molding pressure in step (2) is 600-1500 MPa, for example, it can be 600 MPa, 700 MPa, 800 MPa, 900 MPa, 1000 MPa, 1100 MPa, 1200 MPa, 1300 MPa, 1400 MPa or 1500 MPa, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0075] Preferably, the temperature of the heat treatment in step (3) is 20 to 50°C higher than the melting temperature of the thermoplastic resin, for example, it may be 20°C, 22°C, 23°C, 24°C, 25°C, 30°C, 32°C, 35°C, 40°C, 45°C or 50°C, but is not limited to the listed values, and other values not listed within this range are also applicable.
[0076] Preferably, the heat treatment time is 10 to 30 min, for example, it can be 10 min, 13 min, 15 min, 17 min, 19 min, 22 min, 24 min, 26 min, 28 min or 30 min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0077] Preferably, when the temperature of the heat treatment is ≥250° C., the heat treatment is performed in an inert atmosphere or a vacuum environment.
[0078] Compared with the prior art, the present invention has at least the following beneficial effects:
[0079] (1) The mixed rubber composite powder for recyclable compressed bonded magnets provided by the present invention can enhance the fit between magnetic powders by using mixed rubbers of different particle sizes and using magnetic powders of different particle sizes in mixed rubbers of different particle sizes;
[0080] (2) The recyclable compressed bonded magnet provided by the present invention can be recycled and reused, which solves the problem that thermosetting resin cannot be recycled and reused, and greatly reduces the cost of magnetic powder. When the recycled powder is added at a ratio of 20% after 5 times of recycling, the residual magnetism is reduced by ≤1.42%, and the ring crushing force is reduced by less than 0.72%; when the recycled powder is added at a ratio of 30% after 5 times of recycling, the residual magnetism is reduced by ≤1.73%, and the ring crushing force is reduced by less than 0.81%; when the recycled powder is added at a ratio of 20% after 10 times of recycling, the residual magnetism is reduced by ≤1.46%, and the ring crushing force is reduced by less than 0.74%;
[0081] (3) The preparation method of the recyclable compressed bonded magnet provided by the present invention comprises mixing magnetic powders of different particle sizes with thermoplastic resins respectively, crushing to obtain mixed rubber materials of different particle sizes, and then compressing and molding them, thereby avoiding deformation of the magnets during compression molding and heat treatment. DETAILED DESCRIPTION
[0082] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0083] It should be understood that, in the description of the present invention, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0084] In order to facilitate the final test, the following examples and comparative examples were uniformly pressed into Cylinder and The ring is a circular ring, but the scope of protection of the present invention is not limited thereto, and the ring can be pressed into various shapes and sizes according to actual production needs.
[0085] Example 1
[0086] The present embodiment provides a recyclable compressed bonded magnet, which includes magnetic powder and thermoplastic resin, the mass fraction of the thermoplastic resin in the magnetic powder is 2.0wt%, that is, a is 2.0wt%; the material of the magnetic powder is neodymium iron boron magnetic powder (NdFeB-RM-127 / 72A (GB / T20168-2017)); the thermoplastic resin is polyphenylene sulfide thermoplastic resin (brand SGX-140).
[0087] The preparation method of the recyclable compressed bonded magnet described in this embodiment comprises the following steps:
[0088] (1) The magnetic powder was ground by ball milling with a ball-to-material ratio of 2.5:1 for 40 min. (mass ratio), rotating speed 500r / min, to obtain magnetic powders of target particle size;
[0089] Magnetic powders (NdFeB magnetic powders) with different particle sizes are independently mixed with thermoplastic resin in a V-type mixer for 60 minutes, and then mixed in a single-screw mixer for 15 minutes; the mixed materials are then crushed independently by a vibration crushing and screening machine, with a vibration frequency of 25 Hz and an amplitude of 3 mm. Powders smaller than the sieve particle size fall under the sieve, and those on the sieve continue to be crushed until they are smaller than the sieve particle size, thereby obtaining a mixed rubber composite powder composed of mixed rubbers with different particle sizes;
[0090] The particle sizes and mass distribution of magnetic powders with different particle sizes in the first mixed rubber, the second mixed rubber, the third mixed rubber, the fourth mixed rubber and the fifth mixed rubber are as follows:
[0091] The first mixed rubber particle size is less than 75 μm: the magnetic powder particle size is less than 40 μm 12wt%;
[0092] The second mixed rubber has a particle size of 75-100 μm: the magnetic powder has a particle size of 40-75 μm and 35 wt%;
[0093] The third mixed rubber has a particle size of 100-150 μm: the magnetic powder has a particle size of 75-100 μm, 35 wt%;
[0094] Fourth mixed rubber particle size 150-250 μm: magnetic powder particle size 100-150 μm 18wt%;
[0095] The fifth mixed rubber particle size is 150-250 μm: the magnetic powder particle size is >150 μm 0wt%.
[0096] Moreover, in the first rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 2.02a; in the second rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.35a; in the third rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.65a; in the fourth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.32a.
[0097] (2) The mixed rubber combination powder of step (1) is added with 0.2 wt% zinc stearate and mixed evenly, filled into a mold and compressed at 1000 MPa and room temperature (25° C.), and the compression molding process is performed to form Cylinder and The ring is then demoulded to obtain a bonded magnet magnet blank;
[0098] (3) The bonded magnet formed blank of step (2) is heat treated at 310° C. for 15 min under vacuum conditions in a vacuum drying oven to obtain a recyclable compressed bonded magnet.
[0099] Example 2
[0100] The present embodiment provides a recyclable compressed bonded magnet, which includes magnetic powder and thermoplastic resin, the mass fraction of the thermoplastic resin in the magnetic powder is 1.8wt%, that is, a is 1.8wt%; the material of the magnetic powder is neodymium iron boron magnetic powder (NdFeB-RM-127 / 72A (GB / T20168-2017)); the thermoplastic resin is a polyimide thermoplastic resin (brand TS1450).
[0101] The preparation method of the recyclable compressed bonded magnet described in this embodiment comprises the following steps:
[0102] (1) The magnetic powder was ground by ball milling with a ball-to-material ratio of 3.0:1 for 20 min. (mass ratio), rotating speed 800r / min, to obtain magnetic powders of target particle size;
[0103] Magnetic powders (NdFeB magnetic powders) with different particle sizes are independently mixed with thermoplastic resin in a V-type mixer for 55 minutes, and then mixed in a single-screw mixer for 20 minutes; the mixed materials are then crushed independently by a vibration crushing and screening machine, with a vibration frequency of 25 Hz and an amplitude of 5 mm. Powders smaller than the sieve particle size fall under the sieve, and those on the sieve continue to be crushed until they are smaller than the sieve particle size, thereby obtaining a mixed rubber composite powder composed of mixed rubbers with different particle sizes;
[0104] The particle sizes and mass distribution of magnetic powders with different particle sizes in the first mixed rubber, the second mixed rubber, the third mixed rubber, the fourth mixed rubber and the fifth mixed rubber are as follows:
[0105] The first mixed rubber particle size is less than 75 μm: the magnetic powder particle size is less than 40 μm 10wt%;
[0106] The second mixed rubber material is 75-100 μm: magnetic powder particle size is 40-75 μm 40wt%;
[0107] The third mixed rubber material is 100-150 μm: magnetic powder particle size is 75-100 μm 30wt%;
[0108] Fourth mixed rubber material 150-250 μm: magnetic powder particle size 100-150 μm 19wt%;
[0109] Fifth mixed rubber material 150-250 μm: magnetic powder particle size> 150 μm 1wt%.
[0110] Moreover, in the first rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.6a; in the second rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.5a; in the third rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.6a; in the fourth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.31a; in the fifth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.11a.
[0111] (2) The mixed rubber combination powder of step (1) is mixed with 0.1% zinc stearate and filled into a mold and compressed at 1200 MPa and room temperature (28° C.) to form a Cylinder and The ring is then demoulded to obtain a bonded magnet magnet blank;
[0112] (3) The bonded magnet formed blank of step (2) is heat treated at 270° C. for 30 min under vacuum conditions in a vacuum drying oven to obtain a recyclable compressed bonded magnet.
[0113] Example 3
[0114] The present embodiment provides a recyclable compressed bonded magnet, which includes magnetic powder and thermoplastic resin, the mass fraction of the thermoplastic resin in the magnetic powder is 3.0wt%, that is, a is 3.0wt%; the material of the magnetic powder is neodymium iron boron magnetic powder (NdFeB-RM-127 / 72A (GB / T20168-2017)); the thermoplastic resin is polypropylene thermoplastic resin (brand name P6209).
[0115] The preparation method of the recyclable compressed bonded magnet described in this embodiment comprises the following steps:
[0116] (1) The magnetic powder was ground by ball milling with a ball-to-material ratio of 0.5:1 for 60 min. (mass ratio), rotating speed 300r / min, to obtain magnetic powders of target particle size;
[0117] Magnetic powders (NdFeB magnetic powders) with different particle sizes are independently mixed with thermoplastic resin in a V-type mixer for 65 minutes, and then mixed in a single-screw mixer for 25 minutes; the mixed materials are then crushed independently by a vibration crushing and screening machine, with a vibration frequency of 25 Hz and an amplitude of 1 mm. Powders smaller than the size of the sieve fall under the sieve, and those on the sieve continue to be crushed until they are smaller than the size of the sieve, to obtain a mixed rubber composite powder composed of mixed rubbers with different particle sizes;
[0118] The particle sizes and mass distribution of magnetic powders with different particle sizes in the first mixed rubber, the second mixed rubber, the third mixed rubber, the fourth mixed rubber and the fifth mixed rubber are as follows:
[0119] The first mixed rubber particle size is less than 75 μm: the magnetic powder particle size is less than 40 μm 18wt%;
[0120] The second mixed rubber material is 75-100 μm: magnetic powder particle size is 40-75 μm 30wt%;
[0121] The third mixed rubber material is 100-150 μm: magnetic powder particle size is 75-100 μm 39 wt%;
[0122] Fourth mixed rubber material 150-250 μm: magnetic powder particle size 100-150 μm 12.5 wt%;
[0123] Fifth mixed rubber material 150-250 μm: magnetic powder particle size> 150 μm 0.5wt%.
[0124] Moreover, in the first rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 2.2a; in the second rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.3a; in the third rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.5a; in the fourth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.2a; in the fifth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.1a.
[0125] (2) The mixed rubber combination powder of step (1) is mixed with 0.5% zinc stearate and filled into a mold and compressed at 800 MPa and room temperature (20° C.) to form a Cylinder and The ring is then demoulded to obtain a bonded magnet magnet blank;
[0126] (3) The bonded magnet formed blank of step (2) is heat treated at 200° C. for 10 min in air in a drying oven to obtain a recyclable compressed bonded magnet.
[0127] Example 4
[0128] The present embodiment provides a recyclable compressed bonded magnet, which is the same as Embodiment 1 except that in the first mixed rubber material with a particle size of <75μm, the magnetic powder particle size of <40μm accounts for 8wt% of the total magnetic powder, and in the second mixed rubber material with a particle size of <100μm, the magnetic powder particle size of 40-75μm accounts for 39wt% of the total magnetic powder. Such details will not be repeated here.
[0129] Example 5
[0130] The present embodiment provides a recyclable compressed bonded magnet, which is the same as Embodiment 1 except that in the third mixed rubber material with a particle size of <150μm, the magnetic powder particle size of 75-100μm accounts for 45wt% of the total magnetic powder, and in the fourth mixed rubber material with a particle size of <250μm, the magnetic powder particle size of 100-150μm accounts for 8wt% of the total magnetic powder, and the rest are no longer repeated here.
[0131] Example 6
[0132] This embodiment provides a recyclable compressed bonded magnet, which is the same as Embodiment 1 except that in the first rubber mixture, the mass ratio of thermoplastic resin to magnetic powder is 2.5a, and the remaining thermoplastic resin is adjusted accordingly from the second rubber mixture, and the rest is not repeated here.
[0133] Example 7
[0134] This embodiment provides a recyclable compressed bonded magnet, which is the same as Embodiment 1 except that in the second rubber mixture, the mass ratio of thermoplastic resin to magnetic powder is 0.5a, and the remaining thermoplastic resin is adjusted accordingly from the third rubber mixture, and the rest is not repeated here.
[0135] Comparative Example 1
[0136] This comparative example provides a recyclable compressed bonded magnet. The preparation method of the recyclable compressed bonded magnet is the same as that of Example 1 except that the magnetic powders of different particle sizes in Example 1 are mixed with thermoplastic resin at one time and crushed to obtain mixed rubbers of different particle sizes. The specific steps (1) are as follows:
[0137] (1) The magnetic powder was ground by ball milling with a ball-to-material ratio of 2.5:1 for 40 min. (mass ratio), speed 500r / min, respectively obtain magnetic powders of target particle size; all magnetic powders (NdFeB magnetic powders) of different particle sizes are first mixed with thermoplastic resin in a V-type mixer for 60min, and then mixed in a single-screw mixer for 15min; then a vibrating crushing and screening machine is used to crush the mixed materials, the vibration frequency is 25Hz, the amplitude is 3mm, and the powder smaller than the sieve particle size falls under the sieve, and the powder on the sieve is continuously crushed until it is smaller than the sieve particle size, to obtain a mixed rubber composite powder composed of mixed rubbers of different particle sizes;
[0138] The magnetic powders with different particle sizes and their mass distribution are as follows:
[0139]
[0140] The mixed rubber materials with different particle sizes are as follows: the particle size of the first mixed rubber material is less than 75 μm, the particle size of the second mixed rubber material is less than 100 μm, the particle size of the third mixed rubber material is less than 150 μm, and the particle size of the fourth mixed rubber material is less than 250 μm.
[0141] The remaining steps are the same as those in Example 1 and will not be described again.
[0142] Comparative Example 2
[0143] This comparative example provides a recyclable compressed bonded magnet. The preparation method of the recyclable compressed bonded magnet is the same as that of Example 1 except that magnetic powders of the same particle size are divided into 4 batches and mixed according to different thermoplastic resin ratios to obtain mixed rubber materials of different particle sizes. The specific steps (1) are as follows:
[0144] (1) The magnetic powder was ground by ball milling with a ball-to-material ratio of 2.5:1 for 40 min. (mass ratio), speed 500r / min, respectively obtain magnetic powders of target particle size; the same magnetic powder is divided into 4 batches and independently mixed with thermoplastic resin in a V-type mixer for 60min, and then mixed in a single-screw mixer for 15min; then a vibration crushing and screening machine is used to crush the mixed materials independently, with a vibration frequency of 25Hz and an amplitude of 3mm. The powder smaller than the sieve particle size falls under the sieve, and the powder on the sieve is continuously crushed until it is smaller than the sieve particle size, to obtain a mixed rubber composite powder composed of mixed rubbers with different particle sizes;
[0145] The particle sizes and mass distribution of magnetic powders with different particle sizes in the first mixed rubber material, the second mixed rubber material, the third mixed rubber material and the fourth mixed rubber material are as follows:
[0146] The first mixed rubber particle size is less than 250 μm: the magnetic powder particle size is 40 to 100 μm, 12 wt%;
[0147] The second mixed rubber particle size is less than 250 μm: magnetic powder particle size is 40-100 μm 35wt%;
[0148] The third mixed rubber particle size is less than 250 μm: magnetic powder particle size is 40-100 μm 35wt%;
[0149] The fourth mixed rubber particle size is less than 250 μm: the magnetic powder particle size is 40 to 100 μm, 18 wt%.
[0150] Moreover, in the first rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 2.02a; in the second rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.35a; in the third rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.65a; in the fourth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.32a.
[0151] The remaining steps are the same as those in Example 1 and will not be described again.
[0152] Comparative Example 3
[0153] This comparative example provides a recyclable compressed bonded magnet. The preparation method of the recyclable compressed bonded magnet is the same as that of Example 1 except that the mass ratio of the thermoplastic resin to the magnetic powder in the first, second, third and fourth mixed materials is a, that is, 2.0wt%. The specific steps (1) are as follows:
[0154] (1) The magnetic powder was ground by ball milling with a ball-to-material ratio of 2.5:1 for 40 min. (mass ratio), rotating speed 500r / min, to obtain magnetic powders of target particle size;
[0155] Magnetic powders (NdFeB magnetic powders) with different particle sizes are independently mixed with thermoplastic resin in a V-type mixer for 60 minutes, and then mixed in a single-screw mixer for 15 minutes; the mixed materials are then crushed independently by a vibration crushing and screening machine, with a vibration frequency of 25 Hz and an amplitude of 3 mm. Powders smaller than the sieve particle size fall under the sieve, and those on the sieve continue to be crushed until they are smaller than the sieve particle size, thereby obtaining a mixed rubber composite powder composed of mixed rubbers with different particle sizes;
[0156] The particle sizes and mass distribution of magnetic powders with different particle sizes in the first mixed rubber material, the second mixed rubber material, the third mixed rubber material and the fourth mixed rubber material are as follows:
[0157] The first mixed rubber particle size <75μm: magnetic powder particle size <40μm 12wt%;
[0158] The second mixed rubber has a particle size of 75-100 μm: the magnetic powder has a particle size of 40-75 μm and 35 wt%;
[0159] The third mixed rubber has a particle size of 100-150 μm: the magnetic powder has a particle size of 75-100 μm, 35 wt%;
[0160] The fourth mixed rubber particle size is 150-250 μm: the magnetic powder particle size is 100-150 μm, 18 wt%.
[0161] Furthermore, in the first rubber mixture, the second rubber mixture, the third rubber mixture and the fourth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is a.
[0162] The remaining steps are the same as those in Example 1 and will not be described again.
[0163] Test method: Use a roundness tester to test the initial roundness of the ring, and use an imager to test the initial coaxiality of the ring.
[0164] The deformation data of the above embodiments and comparative examples are shown in Table 1.
[0165] Table 1
[0166]
[0167] From Table 1, we can see the following points:
[0168] (1) It can be seen from Examples 1 to 3 that the recyclable compressed bonded magnet provided by the present invention uses a thermoplastic resin instead of a thermosetting resin, and by designing that the larger the particle size of the magnetic powder in the mixed rubber, the smaller the mass ratio of the magnetic powder to the thermoplastic resin, the better the recyclability of the magnet and the smaller the deformation during the preparation process. The roundness of the ring is within 0.021, and the coaxiality of the ring is within 0.028;
[0169] (2) Combining Example 1 and Examples 4-5, it can be seen that in Example 1, the proportion of magnetic powder particle sizes in the mixed rubber materials with different particle sizes is strictly controlled within a specific range. Compared with the first mixed rubber material with a particle size of <75 μm and a magnetic powder particle size of <40 μm in the total magnetic powder content being relatively low, and the third mixed rubber material with a particle size of <150 μm and a magnetic powder particle size of 75-100 μm in the total magnetic powder content being relatively high, in Example 1, the proportion of magnetic powder particle sizes in the mixed rubber materials with different particle sizes is strictly controlled within a specific range. The circularity of the ring is 0.014, and the coaxiality of the ring is 0.023. The circularity of the rings is as high as 0.052 and 0.043, respectively, and the coaxiality of the rings is as high as 0.049 and 0.063, respectively. This shows that the present invention can further ensure the shape of the recyclable compressed bonded magnet after pressing by preferably mixing a specific amount of magnetic powder of different particle sizes into the mixed rubber of different particle sizes, avoid deformation during the production process, thereby reducing waste caused by subsequent processing and reducing costs;
[0170] (3) Combining Example 1 and Examples 6-7, it can be seen that in Example 1, the mass ratio of the thermoplastic resin to the magnetic powder is strictly controlled within a specific range. Compared with the mass ratio of the thermoplastic resin to the magnetic powder in the first mixed rubber material in Examples 6-7 being 2.5a and the mass ratio of the thermoplastic resin to the magnetic powder in the second mixed rubber material being 0.5a, in Example 1, the mass ratio of the thermoplastic resin to the magnetic powder is strictly controlled within a specific range. The circularity of the ring is 0.014, and the coaxiality of the ring is 0.023. The roundness of the rings is as high as 0.049 and 0.061, respectively, and the coaxiality of the rings is as high as 0.054 and 0.041, respectively. This shows that the present invention can further ensure the shape of the recyclable compressed bonded magnet after pressing by preferably controlling the ratio of magnetic powder to thermoplastic resin to be smaller when the magnetic powder particle size is larger, avoid deformation during the production process, thereby reducing waste caused by subsequent processing and reducing costs;
[0171] (3) Combining Example 1 and Comparative Examples 1 to 3, it can be seen that in Comparative Example 1, the magnetic powders of different particle sizes in Example 1 are mixed with thermoplastic resin at one time, and the final recyclable compressed bonded magnet is severely deformed, and The roundness of the ring is 0.102, and the coaxiality of the ring is 0.118; in Comparative Example 2, magnetic powders of the same particle size are mixed in 4 batches according to different thermoplastic resin ratios, and the final recyclable compressed bonded magnet is severely deformed, and The roundness of the ring is 0.086, and the coaxiality of the ring is 0.097; in the first mixed rubber, the second mixed rubber, the third mixed rubber and the fourth mixed rubber in Comparative Example 3, the mass ratio of thermoplastic resin to magnetic powder is a, that is, 2.0wt%. The final recyclable compressed bonded magnet is severely deformed, the roundness of the ring is 0.073, and the coaxiality of the ring is 0.102. This shows that the present invention avoids deformation of the magnet during compression molding and heat treatment by selecting magnetic powder of different particle sizes and mixing them with thermoplastic resin separately, and controlling the mass ratio of magnetic powder to thermoplastic resin to be different.
[0172] The magnetic properties of the rings in Examples 1 to 7 were tested initially and after being reused for 5 times using a magnetic property tester, and the crushing force of the rings in Examples 1 to 7 was tested initially and after being reused for 5 times using a universal testing machine.
[0173] The recovery performance and crushing force data of the above embodiments and comparative examples are shown in Table 2.
[0174] Table 2
[0175]
[0176] It can be seen from Table 2 that: From Examples 1 to 7, it can be seen that the recyclable compressed bonded magnet provided by the present invention adopts thermoplastic resin instead of thermosetting resin, and not only the crushing force of the ring is ≥131N, which meets the use requirements of the bonded magnetic ring, but also after being recycled for 5 times, when the added proportion of recycled powder is 20%, the residual magnetism is reduced by ≤1.42%, and the crushing force of the ring is reduced by less than 0.72%; after being recycled for 5 times, when the added proportion of recycled powder is 30%, the residual magnetism is reduced by ≤1.73%, and the crushing force of the ring is reduced by less than 0.81%; after being recycled for 10 times, when the added proportion of recycled powder is 20%, the residual magnetism is reduced by ≤1.46%, and the crushing force of the ring is reduced by less than 0.74%, and the recyclability is excellent.
[0177] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A mixed rubber composite powder for recyclable compressed bonded magnets, characterized in that: The mixed rubber composite powder comprises mixed rubbers with different particle sizes, the mixed rubbers comprising magnetic powder and a thermoplastic resin coated on the surface of the magnetic powder; the particle sizes of the magnetic powder in the mixed rubbers with different particle sizes are different; When the particle size of the magnetic powder in any mixed rubber material is larger than the particle size of the magnetic powder in any other mixed rubber material, the mass ratio of the thermoplastic resin to the magnetic powder in the mixed rubber material is smaller than the mass ratio of the thermoplastic resin to the magnetic powder in any other mixed rubber material.
2. The rubber compound powder according to claim 1, characterized in that: The mixed rubber materials with different particle sizes include a first mixed rubber material, a second mixed rubber material, a third mixed rubber material, a fourth mixed rubber material and a fifth mixed rubber material; wherein the particle sizes and mass distributions of the magnetic powder in the first mixed rubber material, the second mixed rubber material, the third mixed rubber material, the fourth mixed rubber material and the fifth mixed rubber material are as follows: The magnetic powder particle size in the first mixed rubber material is less than 40 μm 10-18 wt%; The magnetic powder particle size in the second rubber mixture is 40-75 μm, 30-40 wt%; The magnetic powder particle size in the third mixed rubber material is 75-100 μm 30-40 wt%; The magnetic powder particle size in the fourth mixed rubber material is 100-150 μm and 12-20 wt%; The magnetic powder particle size in the fifth mixed rubber material is >150 μm 0-1wt%; Preferably, the material of the magnetic powder includes any one of NdFeB magnetic powder, SmFeN magnetic powder, NdFeN magnetic powder or SmCo magnetic powder, or a combination of at least two thereof; Preferably, the bulk density of the magnetic powder is 3.0-3.3 g / cm 3 ; Preferably, the tap density of the magnetic powder is 3.5 to 3.9 g / cm 3 .
3. The rubber compound powder according to claim 1, characterized in that: The mass fraction of the thermoplastic resin in the mixed rubber composite powder to the magnetic powder is a, wherein the range of a is 1.8 to 3.0 wt %; Preferably, in the first rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.6a to 2.2a; Preferably, in the second rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 1.1a to 1.5a; Preferably, in the third rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.5a to 0.9a; Preferably, in the fourth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.2a to 0.5a; Preferably, in the fifth rubber mixture, the mass ratio of the thermoplastic resin to the magnetic powder is 0.1a to 0.3a; Preferably, the particle size of the first rubber mixture is less than 75 μm; Preferably, the particle size of the second rubber mixture is 75-100 μm; Preferably, the particle size of the third rubber mixture is 100-150 μm; Preferably, the particle size of the fourth rubber mixture is 150-250 μm; Preferably, the particle size of the fifth rubber mixture is 150-250 μm; Preferably, the bulk density of the mixed rubber is 3.2-3.5 g / cm 3 ; Preferably, the tap density of the mixed rubber is 3.7-4.1 g / cm 3 .
4. The rubber compound powder according to claim 1, characterized in that: The thermoplastic resin includes any one of nylon, polyphenylene sulfide, polyimide or polypropylene, or a combination of at least two of them.
5. A recyclable compressed bonded magnet, characterized in that: The recyclable compressed bonded magnet comprises the mixed rubber composite powder for recyclable compressed bonded magnets as claimed in any one of claims 1 to 4; the recyclable compressed bonded magnet comprises magnetic powder and thermoplastic resin, and the mass fraction of the thermoplastic resin in the magnetic powder is 1.8 to 3.0 wt%.
6. The recyclable compressed bonded magnet according to claim 5, characterized in that: The material of the magnetic powder includes any one of NdFeB magnetic powder, SmFeN magnetic powder, NdFeN magnetic powder or SmCo magnetic powder, or a combination of at least two thereof; Preferably, the thermoplastic resin includes any one of nylon, polyphenylene sulfide, polyimide or polypropylene, or a combination of at least two thereof; Preferably, the recyclable compressed bonded magnet further comprises a lubricant accounting for 0.1 to 0.5 wt% of the total mass of the magnetic powder and the thermoplastic resin; Preferably, the lubricant comprises a stearate, preferably zinc stearate.
7. The recyclable compressed bonded magnet according to claim 5 or 6, characterized in that: The roundness of the recyclable compressed bonded magnet is ≤0.06mm; Preferably, the coaxiality of the recyclable compressed bonded magnet is ≤0.08 mm; Preferably, compared with a brand new recyclable compressed bonded magnet, the residual magnetism of the recyclable compressed bonded magnet after N times of reuse is reduced by <2%, and the crushing force of the magnetic ring is reduced by <1%, wherein N≥1.
8. A method for preparing a recyclable compressed bonded magnet according to any one of claims 5 to 7, characterized in that: The preparation method adopts the mixed rubber combination powder for recyclable compressed bonded magnets as described in any one of claims 1 to 4.
9. The preparation method according to claim 8, characterized in that: The preparation method comprises: (1) Magnetic powders of different particle sizes are mixed with thermoplastic resins and crushed separately to obtain mixed rubber composite powders composed of mixed rubbers of different particle sizes; (2) mixing a lubricant and the mixed rubber powder of step (1), filling the mixture into a mold, and performing compression molding and demolding in sequence to obtain a bonded magnet blank; (3) The bonded magnet formed blank in step (2) is heat treated to obtain a recyclable compressed bonded magnet.
10. The preparation method according to claim 9, characterized in that: The crushing in step (1) is carried out using a vibrating crushing and screening machine; Preferably, before the respective mixing, the preparation method further comprises: grinding the magnetic powder by ball milling or air jet milling; Preferably, the compression molding pressure in step (2) is 600-1500 MPa; Preferably, the temperature of the heat treatment in step (3) is 20 to 50° C. higher than the melting temperature of the thermoplastic resin; Preferably, the heat treatment time is 10 to 30 minutes; Preferably, when the temperature of the heat treatment is ≥250° C., the heat treatment is performed in an inert atmosphere or a vacuum environment.
Citation Information
Cited By
Flexible magnet, adhesive mix powder, preparation method and magnetic device
CN123143168A