Lithium manganese iron phosphate positive electrode slurry as well as preparation method and application thereof
By continuously drying lithium iron manganese phosphate multiple times and mixing it with a binder and conductive agent, the problem of moisture influence during the preparation process of lithium iron manganese phosphate cathode material is solved, and the stability and efficient preparation of the slurry are achieved. , reducing production costs and process complexity, and improving the capacity retention rate of lithium-ion batteries.
Patent Information
- Application Number
- CN202410916185.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
AI Technical Summary
In the process of preparing lithium iron manganese phosphate-graphite soft pack batteries, the lithium iron manganese phosphate cathode material is sensitive to moisture and is prone to gelation, which increases the difficulty of processing the cathode slurry. The existing solutions have complex processes and high costs. problem.
By continuously drying lithium iron manganese phosphate multiple times, combined with the mixing of binder and conductive agent, a lithium iron manganese phosphate cathode slurry with a high solid content is prepared, which avoids gelation of the slurry and simplifies preparation. process and reduce production costs.
The stability and consistency of the slurry is achieved, the drying time is shortened, the production efficiency is improved, the production cost is reduced, and the capacity of the lithium iron manganese phosphate cathode is effectively utilized in the lithium-ion battery and the capacity retention rate is improved.
Smart Images

Figure CN118800904A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ion batteries, and specifically relates to a lithium manganese iron phosphate positive electrode slurry and a preparation method and application thereof. Background Art
[0002] With the explosive development of electric vehicles, 3C electronics, distributed energy storage and other industries, lithium-ion batteries have also developed accordingly. As the next generation of phosphate-based lithium-ion battery cathode materials, lithium iron manganese phosphate has the advantages of high safety and low price of lithium iron phosphate. In addition, due to the presence of manganese, lithium iron manganese phosphate has a 4.1V discharge platform in addition to the 3.6V discharge platform, and its energy density can be 10-20% higher than that of lithium iron phosphate batteries. Therefore, lithium iron manganese phosphate cathode materials have great development potential.
[0003] In the process of preparing lithium iron manganese phosphate-graphite soft-pack batteries, mixing lithium iron manganese phosphate, conductive agent, PVDF, etc. to make lithium iron manganese phosphate positive electrode slurry is the first and most critical step in assembling soft-pack batteries. During the positive electrode homogenization process, the lithium iron manganese phosphate positive electrode slurry is sensitive to moisture and is prone to gelation, which increases the difficulty of positive electrode slurry processing. This is mainly because the alkaline substances generated by the reaction of lithium iron manganese phosphate positive electrode materials with moisture are prone to nucleophilic reactions with the CF bonds on PVDF, resulting in PVDF dehydrogenation and fluorination to form cross-linked conjugated polyenes, that is, gelation. Therefore, solving the effect of moisture on the positive electrode slurry in the preparation of the positive electrode slurry is the key to the preparation of lithium iron manganese phosphate-graphite soft-pack batteries.
[0004] At present, there are two common solutions to the problem of gelation caused by excessive moisture content in the positive electrode slurry: first, adding additives (oxalic acid, moisture inhibitors, molecular sieves, etc.) to the positive electrode slurry, and second, structural design of the lithium iron manganese phosphate particles, such as coating design. These two solutions can effectively reduce the impact of moisture on PVDF during the positive electrode homogenization process, minimize gelation, and reduce the processing difficulty of the positive electrode slurry. However, the introduction of additives requires an additional feeding process, which affects the consistency of the slurry; the introduced additives are inactive substances and have an impact on the overall energy density of the battery. In addition, the design of the coating layer for lithium iron manganese phosphate requires additional process links in the preparation process, which is complicated and increases the processing cost. Summary of the invention
[0005] The purpose of the present invention is to provide a lithium manganese iron phosphate positive electrode slurry and a preparation method and application thereof, so as to solve the technical problems of complex preparation process and high cost when introducing multiple substances during the modification of the existing lithium manganese iron phosphate.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention discloses a method for preparing lithium manganese iron phosphate positive electrode slurry, comprising the following steps:
[0008] After the lithium manganese iron phosphate is subjected to continuous multiple drying treatments, dried lithium manganese iron phosphate is obtained;
[0009] The dried lithium manganese iron phosphate, a binder, a conductive agent and a solvent are mixed to obtain a lithium manganese iron phosphate positive electrode slurry.
[0010] Furthermore, the continuous multiple drying processes include a primary drying process, a secondary drying process and a tertiary drying process performed in sequence.
[0011] Furthermore, the process parameters of the primary drying process are:
[0012] Bake the lithium manganese iron phosphate for 10-60 minutes at a vacuum degree of -5 to -20 kPa and a temperature of 90-130°C.
[0013] Furthermore, the process parameters of the secondary drying treatment are:
[0014] S1: After the primary drying process is completed, the air pressure is raised to normal pressure, and then vacuumed to -5 to -20 kPa, and the above steps are repeated several times, and then baked at 90-130°C for 10-60 minutes;
[0015] S2: Repeat step S1 4-8 times at a frequency of 1-5 minutes to complete the secondary drying process.
[0016] Furthermore, the process parameters of the three drying processes are:
[0017] Maintain a vacuum degree of -5 to -20 kPa and bake at 90-130°C for 8-12 hours.
[0018] Further, after the third drying treatment, the second drying treatment and the third drying treatment are repeated 2-3 times in sequence, and then the heating is stopped and naturally cooled for 1-6 hours to obtain dried lithium manganese iron phosphate;
[0019] The ambient temperature of the natural cooling is 20-25° C., and the air humidity is less than 15%.
[0020] Furthermore, the mass ratio of the dried lithium manganese iron phosphate, the binder and the conductive agent is (90-97): (1-5): (1-5); the solid content of the lithium manganese iron phosphate positive electrode slurry is 40-70wt.%;
[0021] The binder is one or more of polyvinylidene fluoride, polymethyl methacrylate and polytetrafluoroethylene; the solvent is one or more of N-methylpyrrolidone, dimethylformamide and dimethyl sulfoxide;
[0022] The polyvinylidene fluoride is selected from one or more of HSV900, Solvay 5130 and Kynar761A;
[0023] The conductive agent is selected from one or more of SP, CNT and KS-6.
[0024] The invention also discloses lithium manganese iron phosphate positive electrode slurry prepared by the preparation method.
[0025] The invention also discloses application of the lithium iron manganese phosphate positive electrode slurry in a lithium ion battery.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The invention discloses a method for preparing a lithium iron manganese phosphate positive electrode slurry. By performing continuous multiple drying treatments on the lithium iron manganese phosphate, the lithium iron manganese phosphate is baked and dehydrated before being homogenized, so that gelation of the slurry is effectively avoided, and the problems of introducing inactive substances to affect the consistency of the slurry, introducing inactive substances to affect the energy density of the battery core, introducing additives to produce uncontrollable chemical reactions, increasing processing steps, and increasing product costs are solved. Compared with simple drying, the above-mentioned continuous multiple drying treatment method can obtain lithium iron manganese phosphate powder with the same moisture content, and the treatment time required for continuous multiple drying is shorter. Therefore, continuous multiple drying treatments can effectively shorten the drying time, shorten the preparation cycle of soft-pack batteries, thereby improving production efficiency and reducing production costs.
[0028] The present invention also discloses a lithium iron manganese phosphate positive electrode slurry prepared by the above-mentioned preparation method. The lithium iron manganese phosphate positive electrode slurry has the advantages of good slurry stability, high slurry consistency, good slurry fluidity and easy coating processing.
[0029] The present invention also discloses the application of the lithium iron manganese phosphate positive electrode slurry in lithium ion batteries, which effectively exerts the capacity of the lithium iron manganese phosphate positive electrode, reduces the influence of moisture and thus improves the capacity retention rate, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The composite viscosity curves of the embodiments of the present invention and the comparative examples;
[0031] Figure 2 1 is a loss tangent value curve of the embodiment of the present invention and the comparative example;
[0032] Figure 3 This is the constant current charge and discharge curve of Example 6 of the present invention at 1C;
[0033] Figure 4 This is the cycle curve of Example 6 of the present invention at 1C. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0035] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0036] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0037] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0038] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0039] The present invention provides a method for preparing a lithium manganese iron phosphate positive electrode slurry, comprising the following steps:
[0040] Step 1: Place the active material lithium manganese iron phosphate into an oven, heat the oven to 90-130°C, and evacuate the oven to -5 to -20 kPa; after the temperature reaches the set temperature, bake for 10-60 minutes to achieve a primary drying process;
[0041] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to the vacuum degree of step 1, repeat 3-4 times, and bake for 10-60 minutes;
[0042] Step 3: Repeat step 2 4-8 times to achieve secondary drying;
[0043] Step 4: Maintain the vacuum degree of the oven and bake at 90-130°C for 8-12 hours to achieve three drying processes;
[0044] Step 5: Repeat steps 2-4 1-3 times;
[0045] Step 6: Stop heating, cool naturally for 1-6 hours and then standby to obtain dried lithium manganese iron phosphate;
[0046] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0047] Preferably, the oven is one of a vacuum oven, a single-layer oven, a double-layer vacuum oven, and a double-door vacuum oven, and the oven heating rate is 10-40°C / min.
[0048] Preferably, the purity of the nitrogen is 99.999% industrial grade purity, and the moisture content of the nitrogen is less than 60 ppm.
[0049] Preferably, the containing container is one of a glass beaker, a glass crystallization dish and a stainless steel square plate, and the height of the active substance is less than 5 cm.
[0050] Preferably, in step 3, the frequency is once every 1-5 minutes.
[0051] Preferably, the ambient temperature of the natural cooling in step 6 is 20-25° C. and the air humidity is less than 15%.
[0052] Preferably, in step 7, PVDF is selected from one or more of HSV900, Solvay 5130, Kynar761A; the conductive agent is selected from one or more of SP, CNT, KS-6; lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 90-97: 1-5: 1-5; the solid content of the positive electrode slurry is 40-70wt.%.
[0053] The present invention also provides an application of the lithium iron manganese phosphate positive electrode slurry prepared by the above-mentioned preparation method, which is to apply it as a lithium ion battery positive electrode slurry on a roller, and finally wind it into a soft-pack battery; specifically, the lithium iron manganese phosphate positive electrode material, conductive agent, PVDF and NMP are mixed into a positive electrode slurry, and graphite, conductive agent, adhesive and water are mixed into a negative electrode slurry; then after coating, drying, die cutting, rolling, welding the pole ears, the positive and negative pole pieces are obtained, and then the positive and negative pole pieces are wound with the Celegard diaphragm, and after liquid injection, formation, secondary sealing, aging, and chemical connection, they are assembled together to obtain a lithium ion soft-pack battery. The obtained battery is subjected to a constant current charge and discharge test, and the test voltage range is 2.6V-4.35V.
[0054] Preferably, the rheological test is conducted at a temperature of 25° C., the test fixture is a steel circular plate with a diameter of 40 mm, and the test gap is 500-1500 μm.
[0055] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0056] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0057] Example 1
[0058] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0059] Step 1: Put lithium manganese iron phosphate into a glass beaker and put it into a vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature rises to the set temperature, bake for 30 minutes to achieve a primary drying process.
[0060] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0061] Step 3: Repeat step 2 4 times to achieve secondary drying;
[0062] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0063] Step 5: Repeat steps 2-4 once;
[0064] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0065] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0066] Among them, in step 3, the frequency is suction every 5 minutes, the PVDF is HSV900; the conductive agent is SP and CNT, the mass ratio is 1:1; the heating rate of the vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0067] Example 2
[0068] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0069] Step 1: Put lithium manganese iron phosphate into a glass beaker and put it into a single-layer oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature rises to the set temperature, bake for 30 minutes to achieve a primary drying process.
[0070] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0071] Step 3: Repeat step 2 6 times to achieve secondary drying;
[0072] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0073] Step 5: Repeat steps 2-4 once;
[0074] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0075] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0076] Among them, in step 3, the frequency is pumping once every 5 minutes, the PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; the heating rate of the single-layer oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0077] Example 3
[0078] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0079] Step 1: Place lithium manganese iron phosphate in a glass crystallization dish and place it in a double-layer vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature reaches the set temperature, bake for 30 minutes to achieve a primary drying process.
[0080] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0081] Step 3: Repeat step 2 8 times to achieve secondary drying;
[0082] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0083] Step 5: Repeat steps 2-4 once;
[0084] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0085] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0086] Among them, in step 3, the frequency is suction every 5 minutes, the PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; the heating rate of the double-layer vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0087] Example 4
[0088] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0089] Step 1: Place lithium manganese iron phosphate in a glass crystallization dish and place it in a double-door vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature reaches the set temperature, bake for 30 minutes to achieve a primary drying process.
[0090] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0091] Step 3: Repeat step 2 4 times to achieve secondary drying;
[0092] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0093] Step 5: Repeat steps 2-4 twice;
[0094] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0095] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0096] Among them, in step 3, the frequency is suction every 5 minutes, the PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; the heating rate of the double-door vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0097] Example 5
[0098] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0099] Step 1: Place lithium manganese iron phosphate in a glass crystallization dish and place it in a double-door vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature reaches the set temperature, bake for 30 minutes to achieve a primary drying process.
[0100] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0101] Step 3: Repeat step 2 6 times to achieve secondary drying;
[0102] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0103] Step 5: Repeat steps 2-4 twice;
[0104] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0105] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0106] Among them, in step 3, the frequency is suction every 5 minutes, the PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; the heating rate of the double-door vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0107] Example 6
[0108] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0109] Step 1: Place lithium manganese iron phosphate in a glass crystallization dish and place it in a double-door vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature reaches the set temperature, bake for 30 minutes to achieve a primary drying process.
[0110] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0111] Step 3: Repeat step 2 8 times to achieve secondary drying;
[0112] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0113] Step 5: Repeat steps 2-4 twice;
[0114] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0115] Step 7: The dried lithium manganese iron phosphate, polyvinylidene fluoride (PVDF), conductive agent, and N-methylpyrrolidone (NMP) are fully mixed to obtain a positive electrode slurry;
[0116] Among them, in step 3, the frequency is suction every 5 minutes, the PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; the heating rate of the double-door vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0117] Example 7
[0118] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0119] Step 1: Place lithium manganese iron phosphate in a glass crystallization dish and place it in a double-door vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature reaches the set temperature, bake for 30 minutes to achieve a primary drying process.
[0120] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0121] Step 3: Repeat step 2 8 times to achieve secondary drying;
[0122] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0123] Step 5: Repeat steps 2-4 twice;
[0124] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0125] Step 7: fully mixing the dried lithium manganese iron phosphate, polymethyl methacrylate, conductive agent, and dimethyl sulfoxide to obtain a positive electrode slurry;
[0126] Among them, in step 3, the frequency is suction once every 1 minute; the conductive agent is KS-6; the heating rate of the double-door vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 90:5:5; the solid content of the positive electrode slurry is 40wt.%.
[0127] Example 8
[0128] A method for preparing lithium manganese iron phosphate positive electrode slurry comprises the following steps:
[0129] Step 1: Place lithium manganese iron phosphate in a glass crystallization dish and place it in a double-door vacuum oven. Set the oven to 110°C and evacuate to -10kPa. After the temperature reaches the set temperature, bake for 30 minutes to achieve a primary drying process.
[0130] Step 2: introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0131] Step 3: Repeat step 2 8 times to achieve secondary drying;
[0132] Step 4: Maintain the oven vacuum degree of -10kPa and bake at 110°C for 12 hours to achieve three drying processes;
[0133] Step 5: Repeat steps 2-4 twice;
[0134] Step 6: Stop heating, cool naturally for 3 hours and set aside to obtain dried lithium manganese iron phosphate;
[0135] Step 7: The dried lithium manganese iron phosphate, polytetrafluoroethylene, conductive agent, and dimethylformamide are fully mixed to obtain a positive electrode slurry;
[0136] Among them, in step 3, the frequency is suction every 3 minutes; the conductive agent is CNT; the heating rate of the double-door vacuum oven is 10°C / min; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 97:1:5; the solid content of the positive electrode slurry is 55wt.%.
[0137] Comparative Example 1
[0138] Without baking the active material lithium manganese iron phosphate, the lithium manganese iron phosphate positive electrode material, PVDF, a conductive agent, and NMP are directly mixed to obtain a positive electrode slurry; wherein the PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; the lithium manganese iron phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0139] Comparative Example 2
[0140] Step 1, put the active material lithium manganese iron phosphate into an oven, heat the oven to 110°C, and evacuate to -10kPa;
[0141] Step 2: After the temperature reaches the set temperature, bake for 30 minutes;
[0142] Step 3, introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0143] Step 4, repeat step 3 0 times;
[0144] Step 5, maintaining the oven vacuum degree of -10 kPa and baking at 110°C for 12 hours;
[0145] Step 6: Repeat steps 3 to 5 once;
[0146] Step 7, stop heating, and cool naturally for 3 hours for standby use;
[0147] Step 8: Take the lithium iron manganese phosphate positive electrode material obtained in step 7, PVDF, and a conductive agent, add NMP and mix thoroughly to obtain a positive electrode slurry; wherein, PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; lithium iron manganese phosphate positive electrode material: PVDF: conductive agent = 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0148] Comparative Example 3
[0149] Step 1, put the active material lithium manganese iron phosphate into an oven, heat the oven to 110°C, and evacuate to -10kPa;
[0150] Step 2: After the temperature reaches the set temperature, bake for 30 minutes;
[0151] Step 3, introduce nitrogen to raise the pressure to normal pressure, then evacuate to -10 kPa, repeat 3 times, and bake for 30 minutes;
[0152] Step 4, repeat step 3 0 times;
[0153] Step 5, maintaining the oven vacuum degree of -10 kPa and baking at 110°C for 12 hours;
[0154] Step 6: Repeat steps 3 to 5 twice;
[0155] Step 7, stop heating, and cool naturally for 3 hours for standby use;
[0156] Step 8: Take the lithium iron manganese phosphate positive electrode material obtained in step 7, PVDF, and a conductive agent, add NMP and mix thoroughly to obtain a positive electrode slurry; wherein, PVDF is HSV900; the conductive agent is SP and CNT, and the mass ratio is 1:1; lithium iron manganese phosphate positive electrode material: PVDF: conductive agent == 95:2:3; the solid content of the positive electrode slurry is 50wt.%.
[0157] The lithium manganese iron phosphate positive electrode slurries obtained in Examples 1 to 6 and the positive electrode slurries obtained in Comparative Examples 1 and 2 were subjected to viscoelastic rheological tests. Under a fixed shear strain of 2%, the angular frequency range was 0.1 rad / s-10 rad / s, and the composite viscosity (η * ), storage modulus (G') and loss modulus (G'); complex viscosity (η * ) decreases with increasing angular frequency, indicating that the positive electrode slurry is shear-thinned; the loss tangent (tanδ=G” / G') is calculated; the loss tangent <1 indicates a tendency to gelation and is not suitable for coating; the data obtained are compared in Table 1, Figure 1 and Figure 2 As shown in Table 1, the performance comparison of different positive electrode slurries in the embodiment and the comparative example is shown. From Table 1, it can be seen that the comparative example (extending the drying time) is difficult to effectively reduce the moisture content of the powder in a short time. Example 6 (extending the drying time and increasing the number of cycle baking) can reduce the moisture content from 2116.520ppm to 512.763ppm; with the same baking time, comparative example 3 only reduces the moisture content from 2116.520ppm to 2016.755ppm.
[0158] Therefore, the drying process proposed in the present invention can greatly shorten the drying time required for lithium iron manganese phosphate powder, which is of great significance for shortening the preparation cycle of soft-pack batteries and thus improving production efficiency. Sufficient drying (increasing the number of baking cycles) can significantly improve the baking effect and effectively reduce the moisture content of the positive electrode material; the loss tangent value of the positive electrode slurry prepared from the low-moisture positive electrode material (<700ppm) is greater than 1, and can be coated.
[0159] The lithium manganese iron phosphate positive electrode material, conductive agent and PVDF are mixed into positive electrode slurry, and graphite, conductive agent and adhesive are mixed into negative electrode slurry. Then, after coating, drying, die-cutting, rolling and welding of pole ears, positive and negative pole pieces are obtained, and then the positive and negative pole pieces are wound with Celegard separators, and after liquid injection, formation, secondary sealing, aging and chemical connection, they are assembled together to obtain lithium-ion soft-pack batteries. The obtained batteries are subjected to constant current charge and discharge tests, and the test voltage range is 2.6V-4.35V. The capacity retention rate after 500 cycles at 1C is 94.87%. (Table 1)
[0160] Table 1 Performance comparison between the embodiment and the comparative example
[0161]
[0162] Figure 2 The loss tangent curves of the embodiments of the present invention and the comparative example are shown. Figure 2 It can be seen that the loss tangent curve of the comparative example (simple drying, only extending the drying time) is lower than 0.5 as a whole; with the extension of the drying time and the increase in the number of baking cycles, the loss tangent curve of the embodiment increases from around 0.6 as a whole to greater than 1.0 as a whole. The above results show that due to the improvement of the drying process, the moisture content of the lithium manganese iron phosphate powder is reduced, and the rheological properties of the slurry made from the lithium manganese iron phosphate powder are improved accordingly. In Example 6, the slurry has good fluidity and is easy to coat and process.
[0163] Figure 3 The constant current charge and discharge curve of Example 6 of the present invention at 1C is shown in FIG. Figure 3 It can be seen that due to the high water content of the lithium manganese iron phosphate powder in the comparative example and some examples, the slurry obtained from the powder has poor fluidity and is difficult to process and coat, and cannot be made into a battery cell for electrochemical testing. The powder of Example 6 has a low water content, and the obtained slurry has good fluidity and can be processed and coated to make a battery cell. Figure 3 The constant current charge and discharge curve of Example 6 of the present invention at 1C is shown in FIG. Figure 3 It can be seen that the charge and discharge curves of the battery cell are smooth, indicating that the slurry has good consistency and the slurry and the current collector are well bonded without falling off; the battery cell has two discharge platforms at ~3.8V and ~3.2V, indicating that the capacity of the main material of lithium manganese iron phosphate is effectively utilized.
[0164] Figure 4 is the cycle curve of Example 6 of the present invention at 1C, from Figure 4It can be seen that the battery cell is stable in charge and discharge; the discharge capacity of the battery cell can reach 1.345Ah, which is 89.7% of the designed capacity; the capacity retention rate is 94.87% after 500 cycles at 1C. The above results show that improving the baking process can not only reduce the difficulty of slurry coating processing and improve production efficiency, but also effectively exert the capacity of lithium manganese iron phosphate cathode, reduce the influence of moisture and thus improve the capacity retention rate.
[0165] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing lithium manganese iron phosphate positive electrode slurry, characterized in that: The following steps are involved: After the lithium manganese iron phosphate is subjected to continuous multiple drying treatments, dried lithium manganese iron phosphate is obtained; The dried lithium manganese iron phosphate, a binder, a conductive agent and a solvent are mixed to obtain a lithium manganese iron phosphate positive electrode slurry.
2. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 1, characterized in that: The continuous multiple drying processes include a primary drying process, a secondary drying process and a tertiary drying process performed in sequence.
3. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 2, characterized in that: The process parameters of the primary drying process are: Bake the lithium manganese iron phosphate for 10-60 minutes at a vacuum degree of -5 to -20 kPa and a temperature of 90-130°C.
4. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 3, characterized in that: The process parameters of the secondary drying process are: S1: After the primary drying process is completed, the air pressure is raised to normal pressure, and then vacuumed to -5 to -20 kPa, and the above steps are repeated several times, and then baked at 90-130°C for 10-60 minutes; S2: Repeat step S1 4-8 times at a frequency of 1-5 minutes to complete the secondary drying process.
5. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 4, characterized in that: The process parameters of the three drying processes are: Maintain a vacuum degree of -5 to -20 kPa and bake at 90-130°C for 8-12 hours.
6. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 5, characterized in that: After the third drying treatment, the second drying treatment and the third drying treatment are repeated 2-3 times in sequence, and then the heating is stopped and the mixture is naturally cooled for 1-6 hours to obtain dried lithium manganese iron phosphate; The ambient temperature of the natural cooling is 20-25° C., and the air humidity is less than 15%.
7. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 1, characterized in that: The mass ratio of the dried lithium manganese iron phosphate, the binder and the conductive agent is (90-97): (1-5): (1-5); the solid content of the lithium manganese iron phosphate positive electrode slurry is 40-70wt.%; The binder is one or more of polyvinylidene fluoride, polymethyl methacrylate and polytetrafluoroethylene; the solvent is one or more of N-methylpyrrolidone, dimethylformamide and dimethyl sulfoxide.
8. The method for preparing a lithium iron manganese phosphate positive electrode slurry according to claim 7, characterized in that: The polyvinylidene fluoride is selected from one or more of HSV900, Solvay 5130 and Kynar761A; The conductive agent is selected from one or more of SP, CNT and KS-6.
9. A lithium manganese iron phosphate positive electrode slurry, characterized in that: The preparation method is described in any one of claims 1 to 8.
10. Use of the lithium iron manganese phosphate positive electrode slurry according to claim 9 in lithium ion batteries.