Surface material for absorbent article
By using a multi-layer structure and metal oxide antibacterial agents combined with fibers in the surface materials of absorbent articles, the problem of antibacterial agents not being easily soluble in water is solved, achieving effective antibacterial effects and balancing resident skin bacteria, and reducing costs.
Patent Information
- Application Number
- CN202380024876.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2023-05-23
- Publication Date
- 2024-10-18
AI Technical Summary
Since the antibacterial agents in existing absorbent articles are not easily soluble in water, the antibacterial effect cannot be fully exerted before urine and other excretion fluids penetrate the surface materials, and the occurrence of skin rashes and other skin problems cannot be effectively suppressed.
A surface material with a multi-layer structure is used, in which there are multiple convex and concave parts on the side of the skin. The inside of the convex part is a hollow part containing metal oxide antibacterial agent and fiber. By mixing the metal oxide antibacterial agent into the surface material, it makes it It is distributed in the fiber to prevent it from moving together with the excrement, ensuring that it remains in the surface material, and through the design of the concave and convex structure and fiber lamination, the frequency of contact between the antibacterial agent and the excrement is increased.
It achieves effective retention and high-frequency contact of antibacterial agents, significantly inhibits bacterial reproduction and skin problems caused by excrement, reduces the use of metal oxide antibacterial agents, maintains the balance of resident bacteria in the skin, and reduces costs.
Smart Images

Figure CN118804731A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a surface material for absorbent articles such as disposable diapers. Background Art
[0002] When wearing absorbent articles such as disposable diapers, sanitary napkins, panty liners (vaginal discharge sheets), and incontinence pads, rashes may sometimes occur on the skin due to stuffiness, etc. Therefore, in order to suppress the occurrence of rashes, an absorbent article using an antibacterial agent in the absorbent article has been proposed.
[0003] For example, Patent Documents 1 and 2 describe absorbent articles in which an antimicrobial agent is mixed into fibers constituting a surface material that comes into contact with the wearer's skin.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2006-55187
[0007] Patent Document 2: Japanese Patent Application Publication No. 2021-52938 Summary of the invention
[0008] A surface material of an absorbent article according to one embodiment of the present invention has a skin side and a non-skin side.
[0009] The skin side surface has a plurality of convex portions and a plurality of concave portions located between the plurality of convex portions.
[0010] The surface material constitutes the upper layer of the skin side and constitutes the non-skin side.
[0011] The convex portion has a hollow portion therein, and the hollow portion is located between the upper layer and the lower layer.
[0012] The fibers constituting the non-skin side of the upper layer forming the hollow portion and the fibers constituting the skin side of the upper layer include metal oxide antimicrobial agent-blended fibers, and the metal oxide antimicrobial agent-blended fibers are fibers containing a metal oxide antimicrobial agent.
[0013] An absorbent article according to one aspect of the present invention includes an absorbent body and a surface material located on the skin-facing side of the absorbent body.
[0014] The surface material has a skin side and a non-skin side.
[0015] The skin side of the surface material has a plurality of protrusions and a plurality of recesses between the plurality of protrusions.
[0016] The surface material constitutes the upper layer of the skin side and constitutes the non-skin side.
[0017] The convex portion has a hollow portion therein, and the hollow portion is located between the upper layer and the lower layer.
[0018] The fibers constituting the non-skin side of the upper layer forming the hollow portion and the fibers constituting the skin side of the upper layer include metal oxide antimicrobial agent-blended fibers, and the metal oxide antimicrobial agent-blended fibers are fibers containing a metal oxide antimicrobial agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The figure shows an example of a disposable diaper as one embodiment of the absorbent article of the present invention, and is a schematic plan view of the skin side (surface material side) showing a state in which elastic members of each part are stretched and developed in a planar shape.
[0020] Figure 2 It is along Figure 1 A schematic cross-sectional view of the absorbent article cut along line II-II.
[0021] Figure 3 This is a schematic cross-sectional view showing an enlarged portion of a surface material constituting a part of the disposable diaper.
[0022] Figure 4 This is a perspective view of a metal oxide antimicrobial agent compounded fiber used in the surface material of the embodiment. DETAILED DESCRIPTION
[0023] In absorbent articles using antimicrobial agents, the antimicrobial agents are not easily soluble in water, so that excretion fluids such as urine pass through the front sheet (surface material) before the antimicrobial effect is fully exerted, resulting in a technical problem that it is difficult to exhibit an effective antimicrobial effect.
[0024] The present invention relates to a surface material of an absorbent article capable of exhibiting an effective antibacterial effect.
[0025] Hereinafter, an absorbent article having the surface material of the present invention will be described with reference to the drawings, taking a disposable diaper as an example.
[0026] <Overall structure of disposable diapers>
[0027] Figure 1 The disposable diaper 1 of the present embodiment shown is a so-called open-type disposable diaper. In addition, the surface material of the present invention is not limited to the open-type disposable diaper, and can also be applied to a briefs type disposable diaper.
[0028] The disposable diaper 1 and each component constituting the disposable diaper 1 have a longitudinal direction X corresponding to the front-back direction of the wearer and a transverse direction Y corresponding to the left-right direction of the wearer and perpendicular to the longitudinal direction X. In addition, the disposable diaper 1 and each component constituting the disposable diaper 1 have a thickness direction Z perpendicular to both the longitudinal direction X and the transverse direction Y.
[0029] In this specification, the skin side of each structure refers to the side located on the skin side of the wearer when the disposable diaper is worn. The non-skin side of each structure refers to the side located on the opposite side to the skin side of the wearer when the disposable diaper is worn. In addition, with respect to the thickness direction Z, the side close to the skin of the wearer when worn is sometimes referred to as the upper side, and the side close to the clothes being worn is sometimes referred to as the lower side.
[0030] Hereinafter, the disposable diaper 1 is referred to as a diaper 1 .
[0031] In addition, in this embodiment, although the disposable diaper of belt type is mentioned as an example, it is also applicable to the disposable diaper of underpants type, sanitary napkin, sanitary pad, and incontinence pad.
[0032] like Figure 1 As shown, the diaper 1 is divided into an abdominal region A located on the abdominal side in the longitudinal direction X, a dorsal region B located on the dorsal side in the longitudinal direction X, and a crotch region C located between the abdominal region A and the dorsal region B.
[0033] The back region B includes side portions protruding outwardly from the crotch region C in the left and right transverse directions Y. Fastening tapes 9 are provided at the side edges of the side portions in the transverse directions Y. Similarly, the ventral region A includes side portions protruding outwardly from the crotch region C in the left and right transverse directions Y.
[0034] A landing tape (not shown) for bonding the hook-and-loop fastener 9 is provided on the non-skin side of the ventral region A. The landing tape is formed of a female member of a mechanical hook-and-loop fastener. The hook-and-loop fastener 9 has a fixing portion 91 formed of a male member of a mechanical hook-and-loop fastener.
[0035] The crotch region C is narrower than the ventral region A and the dorsal region B to form a leg circumference that tapers inwardly in the transverse direction Y, and is disposed in the crotch region including the wearer's urinary area and anus when worn.
[0036] Here, "when worn" means a state where a suitable wearing position as generally assumed is maintained.
[0037] like Figure 1 and 2As shown, the diaper 1 has a surface material (top sheet) 2, a back material (back sheet) 3, an absorbent body 4, a side sheet 5, a pair of hook and loop tapes 9, an intermediate sheet 7, and a leakproof sheet 8. The diaper 1 has a structure in which the back material 3, the leakproof sheet 8, the absorbent body 4, the intermediate sheet 7, and the surface material 2 are stacked in the thickness direction Z. These structures are joined to each other by a known joining method such as a hot melt adhesive.
[0038] The absorber 4 extends along the longitudinal direction X and is disposed between the surface material 2 and the back material 3. That is, the absorber 4 is disposed on the non-skin side of the surface material 2. The absorber 4 absorbs liquid excrement (hereinafter sometimes referred to as "liquid" or "excrement") such as water contained in urine or feces of the wearer from one side of the surface material 2 and diffuses it inside, thereby retaining the liquid.
[0039] The absorbent body 4 includes an absorbent core 40 and a core wrap 41 .
[0040] The absorbent core 40 is mainly composed of an absorbent material capable of retaining liquid. Specifically, the absorbent core 40 has a structure including a hydrophilic fiber stack, a structure including an absorbent polymer supported by the stack, or a structure including only a water-absorbent polymer.
[0041] The core wrap 41 covers the absorbent core 40 and has a function of, for example, maintaining the shape of the absorbent core 40. The core wrap 41 is formed of, for example, a thin and soft paper like tissue paper or a liquid-permeable nonwoven fabric.
[0042] The surface material 2 is arranged to contact the skin of the wearer when the diaper 1 is worn. The surface material 2 is arranged on the skin side 4a side (the upper side in the thickness direction Z) of the absorbent body 4, for example, the central part in the transverse direction Y constituting the skin side of the diaper 1. The surface material 2 is constituted as a liquid-permeable sheet, and is formed by nonwoven fabric composed of synthetic fibers or natural fibers.
[0043] The surface material 2 has a skin side 2a and a non-skin side 2b.
[0044] The details of the surface material 2 will be described later.
[0045] An intermediate sheet 7 may be provided between the surface material 2 and the absorbent body 4. Nonwoven fabrics obtained by various manufacturing methods may be used as the intermediate sheet 7. The intermediate sheet 7 is provided from the viewpoints of improving the permeability of liquid from the surface material 2 to the absorbent body 4, preventing the liquid absorbed by the absorbent body 4 from returning to the surface material 2, and the like.
[0046] The back material 3 is arranged on the non-skin side (below the thickness direction Z) of the absorbent body 4, for example, constituting almost the entire non-skin side of the diaper 1, and constituting the outer cover of the diaper 1 when worn. The back material 3 preferably has leakproof properties, for example, it is formed of a sheet having functions such as poor liquid permeability, water vapor permeability, and water repellency.
[0047] A pair of side sheets 5 are arranged on the transverse Y side of the surface material 2, for example, the transverse Y side constituting the skin side of the diaper 1. It is desirable that the side sheets 5 have leakproof properties, for example, they are formed of sheets having functions such as poor liquid permeability, water vapor permeability, and water repellency. In the pair of side sheets 5, the transverse Y central portion side overlaps with the surface material 2 and is arranged, and the transverse Y side extends to the outside of the surface material 2 and is bonded to the back material 3.
[0048] In the diaper 1, the side sheets 5 are provided with thread-like or belt-like elastic members 50 to constitute a three-dimensional gathers forming sheet.
[0049] The leakage-proof sheet 8 is made of a liquid-impermeable or poorly liquid-permeable resin film, and covers the skin-side surface of the back material 3 .
[0050] <Surface material>
[0051] The surface material 2 will be described.
[0052] [Abstract composition of surface materials]
[0053] The surface material 2 of this embodiment is a concave-convex surface material having a concave-convex surface. Figure 3 As shown, the skin side 2a is a concave-convex surface provided with a plurality of hollow convex portions 33 and a plurality of concave portions 34, and the non-skin side 2b is a flat surface.
[0054] Since the skin side surface 2a is a concavoconvex surface, the skin side surface 2a of the surface material 2 partially contacts the skin when worn. That is, when worn, the surface material 2 is easily partially contacted with the skin, and more specifically, the top of the convex part 33 and the area near it are easy to contact the skin. As a result, the stickiness, stuffiness, and irritation caused by friction caused by the entire surface of the skin side surface 2a of the surface material 2 contacting the skin can be reduced, and skin problems such as inflammation, eczema, or skin rash can be suppressed.
[0055] In addition, the term "flat" in this specification means that the surface is flat without any concavities and convexities on a macroscopic scale, and since the surface is made of fibers, relatively small concavities and convexities that may occur are allowed. For example, concavities and convexities with a difference of less than 0.3 mm between the top of a convex portion and the bottom of a concave portion in the thickness direction are allowed.
[0056] like Figure 3As shown, the surface material 2 is composed of a lower layer LL and an upper layer UL formed on the lower layer LL. The lower layer LL constitutes the non-skin side 2b of the surface material 2. The upper layer UL constitutes the skin side 2a of the surface material 2.
[0057] like Figure 3 As shown, the surface material 2 has a plurality of concave portions 34 and a plurality of convex portions 33 on its skin side 2a. A plurality of convex portions 33 are formed on one surface of the skin side 2a. The convex portions 33 are configured to protrude toward the skin side, and concave portions 34 that are recessed toward the non-skin side are formed between the convex portions 33.
[0058] The convex portion 33 includes a flat lower layer LL portion and an upper layer UL portion that protrudes in a dome shape toward the skin of the wearer when the diaper 1 is manufactured.
[0059] The interior of the convex portion 33 is hollow, and the convex portion 33 has a hollow portion 10. The hollow portion 10 is a space located between the upper layer UL and the lower layer LL and surrounded by the non-skin side surface ULb of the upper layer UL and the skin side surface LLa of the lower layer LL.
[0060] The plurality of protrusions 33 are formed, for example, in a staggered grid pattern. The plurality of recesses 34 are also formed in a staggered grid pattern. The shapes and arrangements of the protrusions 33 and recesses 34 are not particularly limited.
[0061] The surface material 2 has a pressed area 52a where the fibers of the upper layer UL and the lower layer LL are compressed and joined by local pressing, and a raised area 52b where the upper layer UL and the lower layer LL are not pressed and the upper layer UL is raised toward the skin side to form a convex portion 33.
[0062] The concave portion 34 is formed by the pressed area 52a and the side surface of the convex portion 33 located around the pressed area 52a. The concave portion 34 has a space 30 that can easily store excrement.
[0063] The pressing of the pressing area 52a may be performed by a method accompanied by melting of the fiber material constituting the surface material 2 or by a method not accompanied by melting of the fiber material. As the pressing process accompanied by melting of the fiber material, specifically, known embossing processes such as embossing with heating and ultrasonic embossing can be cited, and the pressing area 52a is also referred to as an embossed portion.
[0064] like Figure 3 As shown, in the surface material 2, the upper layer UL is formed by laminating a first layer 21 and a second layer 22 arranged in this order from the skin side to the non-skin side (from top to bottom in the figure).
[0065] The skin side surface of the first layer 21 constitutes the skin side surface ULa of the upper layer UL. The skin side surface ULa constitutes the skin side surface 2a of the surface material. The skin side surface ULa is a surface that can directly contact the skin of the wearer.
[0066] The non-skin side surface of the second layer 22 constitutes the non-skin side surface ULb of the upper layer UL.
[0067] like Figure 3 As shown, in the surface material 2, the lower layer LL includes the third layer 23 constituting the skin side LLa of the lower layer LL. In the surface material 2 of this embodiment, the lower layer LL has a single-layer structure, the lower layer LL is composed of the third layer 23, and the skin side LLa of the lower layer LL can be referred to as the skin side 23a of the third layer 23. Hereinafter, the lower layer LL will be referred to as the third layer 23, and the skin side LLa of the lower layer LL will be referred to as the skin side 23a of the third layer 23 for explanation.
[0068] The first layer 21, the second layer 22, and the third layer 23 are each composed of a sheet of a fiber material. As the sheet, for example, various nonwoven fabrics such as nonwoven fabrics produced by a carding method, spunbonded nonwoven fabrics, meltblown nonwoven fabrics, spunlaced nonwoven fabrics, and needle-punched nonwoven fabrics can be used.
[0069] [Composition of the first layer]
[0070] like Figure 3 As shown, the first layer 21 is composed of a fiber assembly, and the fibers constituting the first layer 21 are referred to as first fibers 61. The first fibers 61 are metal oxide antimicrobial agent compounded fibers containing a metal oxide antimicrobial agent. In this embodiment, the case where all of the first fibers 61 constituting the first layer 21 are metal oxide antimicrobial agent compounded fibers is cited as an example for explanation. Hereinafter, the first fibers 61 are referred to as first metal oxide antimicrobial agent compounded fibers 61 for explanation. The metal oxide antimicrobial agent mixed in the metal oxide antimicrobial agent compounded fibers is shown as described later. Figure 4 The symbol 6 is hereinafter referred to as metal oxide antibacterial agent 6.
[0071] In addition, the first layer 21 may be configured to contain both metal oxide antimicrobial agent compounded fibers and metal oxide antimicrobial agent non-compounded fibers not compounded with a metal oxide antimicrobial agent.
[0072] The first metal oxide antimicrobial agent compounding fiber 61 is formed by mixing the metal oxide antimicrobial agent 6 into the fiber. In the first metal oxide antimicrobial agent compounding fiber 61, the metal oxide antimicrobial agent can be effectively prevented from falling off from the fiber, compared with the case where the antimicrobial agent is attached to the fiber by spraying, coating, etc. By mixing the metal oxide antimicrobial agent 6 into the fiber, the metal oxide antimicrobial agent 6 is not easy to move to other layers together with the excrement, and is easy to remain on the surface material 2. The same is true for the second metal oxide antimicrobial agent compounding fiber 621 described later.
[0073] The details of the metal oxide antimicrobial agent compounded fiber and the metal oxide antimicrobial agent non-compounded fiber will be described later.
[0074] [Composition of the second layer]
[0075] The second layer 22 is composed of a fiber assembly, and the fibers constituting the second layer 22 are referred to as second fibers 62. The second fibers 62 include metal oxide antimicrobial agent compounding fibers 621 (hereinafter referred to as second metal oxide antimicrobial agent compounding fibers 621) as fibers containing the metal oxide antimicrobial agent 6 and metal oxide antimicrobial agent non-compounding fibers 622 (hereinafter referred to as second metal oxide antimicrobial agent non-compounding fibers 622). The second metal oxide antimicrobial agent compounding fibers 621 are composed by mixing the metal oxide antimicrobial agent 6 into the fibers.
[0076] [Composition of the third layer]
[0077] The third layer 23 is composed of a fiber assembly, and the fibers constituting the third layer 23 are referred to as third fibers 63. In this embodiment, the case where all the third fibers 63 constituting the third layer 23 are non-metal oxide antibacterial agent-matched fibers is cited as an example for explanation. Hereinafter, the third fibers 63 are referred to as third metal oxide antibacterial agent-non-matched fibers 63 for explanation. In addition, the third layer 23 can be configured to include both metal oxide antibacterial agent-non-matched fibers and metal oxide antibacterial agent-matched fibers.
[0078] [Overall composition of surface materials]
[0079] exist Figure 3 In the figure, the first metal oxide antimicrobial agent compounding fiber 61 constituting the first layer 21 is indicated by a line with a full interior. The second fiber 62 constituting the second layer 22 (including the second metal oxide antimicrobial agent compounding fiber 621 and the second metal oxide antimicrobial agent non-combining fiber 622) is indicated by a line with a slash inside. The third metal oxide antimicrobial agent non-combining fiber 63 constituting the third layer 23 is indicated by a line with a white interior and only an outline. In addition, Figure 4 In the figure, the small circle with a white interior and a small circle with a black interior schematically represent the fusion zone between the fibers.
[0080] In the surface material 2 of the present embodiment, the skin side ULa and the non-skin side ULb of the upper layer UL are composed of metal oxide antibacterial agent compounding fibers containing a metal oxide antibacterial agent mixed therein. On the other hand, the skin side LLa of the lower layer LL is composed of metal oxide antibacterial agent non-compounding fibers without a metal oxide antibacterial agent mixed therein.
[0081] [Antibacterial agent]
[0082] As the metal oxide antibacterial agent, zinc oxide, silver oxide, aluminum oxide, calcium oxide, magnesium oxide, copper oxide, etc. can be used. These metal oxide antibacterial agents can be used alone or in combination of two or more. Among these, from the perspective of antimicrobial property, safety, and price, it is preferred to contain zinc oxide.
[0083] From the viewpoint that the metal oxide antimicrobial agent is not easily transferred to other layers, the metal oxide antimicrobial agent is preferably poorly soluble in water or insoluble in water.
[0084] In the present embodiment, as the metal oxide antimicrobial agent, an example of using poorly water-soluble zinc oxide is given.
[0085] There are many different opinions on the antibacterial mechanism of zinc oxide. For example, zinc ions destabilize bacterial cell membranes and induce cell death; zinc oxide reacts with water and the hydrogen peroxide produced inhibits bacteria.
[0086] Since zinc oxide is poorly soluble in water, it is not easy to move to other layers such as the absorbent body 4 in the surface material 2 together with the excrement moving in the thickness direction Z, and is likely to remain in the surface material 2. In addition, since zinc oxide is mixed into the fiber, it is more likely to remain in the surface material 2.
[0087] In this embodiment, the skin side ULa and non-skin side ULb of the upper layer UL are constructed to contain metal oxide antibacterial agent compounding fibers, and in the surface material 2, the metal oxide antibacterial agent is easily retained on the skin side ULa and non-skin side ULb of the upper layer UL.
[0088] [Metal oxide antimicrobial agent compounded fiber]
[0089] The first metal oxide antimicrobial agent-blended fiber 61 and the second metal oxide antimicrobial agent-blended fiber 621 can be obtained, for example, by spinning a synthetic resin into which a metal oxide antimicrobial agent is pre-mixed.
[0090] The first metal oxide antimicrobial agent compounded fiber 61 and the second metal oxide antimicrobial agent compounded fiber 621 can be, for example, a single fiber composed of one synthetic resin (thermoplastic resin) or a blended polymer obtained by mixing two or more synthetic resins, or can also be a composite fiber. The composite fiber referred to here refers to a synthetic fiber (thermoplastic fiber) obtained by combining two or more synthetic resins of different components using a spinning head and spinning them simultaneously, and the multiple components are continuous structures in the length direction of the fiber, and are bonded to each other in a single fiber. The composite fiber has a core-sheath type, a parallel type, and the like.
[0091] From the viewpoint of effectively expressing the antimicrobial effect, it is preferred that the metal oxide antimicrobial agent is exposed on the surface of the metal oxide antimicrobial agent compounded fiber.
[0092] From the perspective of effectively exposing the metal oxide antimicrobial agent on the fiber surface, the first metal oxide antimicrobial agent-blended fiber 61 and the second metal oxide antimicrobial agent-blended fiber 621 are preferably core-sheath type fibers.
[0093] like Figure 4 As shown, the first metal oxide antimicrobial agent compounded fiber 61 (second metal oxide antimicrobial agent compounded fiber 621) mixed with the metal oxide antimicrobial agent 6 has a core portion 61C (621C) and a sheath portion 61S (621S). The metal oxide antimicrobial agent 6 is compounded only in the sheath portion 61S (621S). In this way, by compounding the metal oxide antimicrobial agent 6 only in the sheath portion 61S (621S), the metal oxide antimicrobial agent 6 can be easily exposed on the fiber surface with a small content of the metal oxide antimicrobial agent.
[0094] From the perspective of effectively and efficiently exerting the effect of the metal oxide antibacterial agent 6 in preventing skin problems and maintaining a good balance of resident bacteria in the skin, the proportion of the metal oxide antibacterial agent 6 in the core-sheath type metal oxide antibacterial agent compounded fiber (the first metal oxide antibacterial agent compounded fiber 61 or the second metal oxide antibacterial agent compounded fiber 621) is preferably 0.05 mass % or more, more preferably 0.1 mass % or more, preferably 2.5 mass % or less, more preferably 2.0 mass % or less, preferably 0.05 mass % or more and 2.5 mass % or less, more preferably 0.1 mass % or more and 2.0 mass % or less.
[0095] The method for calculating the proportion of the metal oxide antimicrobial agent in the metal oxide antimicrobial agent-blended fiber will be described later.
[0096] In addition, in the core-sheath type metal oxide antimicrobial agent compounded fiber (the first metal oxide antimicrobial agent compounded fiber 61 or the second metal oxide antimicrobial agent compounded fiber 621), from the viewpoint of exposing the metal oxide antimicrobial agent 6 on the fiber surface, effectively and efficiently exerting the effect of preventing skin problems brought about by the metal oxide antimicrobial agent 6, and maintaining a good balance of resident bacteria in the skin, it is preferred that the metal oxide antimicrobial agent be contained only in the sheath portion. In the core-sheath type metal oxide antimicrobial agent compounded fiber (the first metal oxide antimicrobial agent compounded fiber 61 or the second metal oxide antimicrobial agent compounded fiber 621), from the above viewpoint, the proportion of the metal oxide antimicrobial agent 6 in the resin constituting the sheath portion (61S or 621S) is preferably 0.1 mass % to 5.0 mass %, and more preferably 0.2 mass % to 4.0 mass %.
[0097] As the core-sheath type first metal oxide antimicrobial agent compound fiber 61 (second metal oxide antimicrobial agent compound fiber 621) of the raw material fiber, for example, the following fiber can be used, wherein the core 61C (62C) is composed of PET (polyethylene terephthalate) and / or PP (polypropylene), and the sheath 61S (62S) is composed of PE (polyethylene) mixed with a metal oxide antimicrobial agent (zinc oxide), and the core-sheath ratio is 20 / 80 to 80 / 20 in terms of mass ratio. The core-sheath ratio represents the mass ratio of the resins constituting the core and the sheath (core / sheath).
[0098] The particle size of the metal oxide antimicrobial agent 6 containing a metal oxide is appropriately set from the perspective of the thickness of the fiber (the first metal oxide antimicrobial agent compounded fiber 61 and the second metal oxide antimicrobial agent compounded fiber 621) in which the metal oxide antimicrobial agent is compounded and the ease of mixing the metal oxide antimicrobial agent into the fiber. Generally, the average particle size of the metal oxide antimicrobial agent is the cumulative volume 50% volume cumulative particle size D obtained by the laser diffraction scattering particle size distribution measurement method. 50 Indicates that it is greater than 1.0 μm and less than 7 μm.
[0099] [Antibacterial agent non-compounded fiber]
[0100] The second metal oxide antimicrobial agent-free fiber 622 and the third metal oxide antimicrobial agent-free fiber 63 may be single fibers composed of, for example, one synthetic resin (thermoplastic resin) or a blended polymer obtained by mixing two or more synthetic resins, or may be composite fibers.
[0101] The second metal oxide antimicrobial agent non-compounded fiber 622 and the third metal oxide antimicrobial agent non-compounded fiber 63 are, for example, core parts composed of PET (polyethylene terephthalate) and / or PP (polypropylene), sheath parts composed of PE (polyethylene), and the core-sheath ratio is 20 / 80 to 80 / 20 in terms of mass ratio. Core-sheath type composite fibers.
[0102] [Hollow and recessed parts]
[0103] As described above, the convex portion 33 has the hollow portion 10 therein. In the hollow portion 10, the excrement liquid supplied to the surface material 2 and passed through the upper layer UL is likely to be temporarily retained.
[0104] In addition, in the concave portion 34, due to its concave shape, excrement is easily retained. In addition, in the surface material 2 of this embodiment, the pressing area 52a and its vicinity constituting a part of the concave portion 34 are compared with their surroundings (the portion roughly corresponding to the convex area 52b that has not been pressed), due to the fusion or compression of the fibers, the fiber density becomes higher and the distance between the fibers becomes smaller. Therefore, the pressing area 52a and its vicinity are easy to introduce excrement and difficult to penetrate due to the difference in fiber density with their surroundings, and the excrement is more likely to be retained in the concave portion 34.
[0105] Thus, the excrement from the wearer is easily retained in the hollow portion 10 and the recessed portion 34 .
[0106] In the recessed portion 34 , the skin-side surface ULa of the upper layer UL is a surface that directly contacts the excrement retained in the recessed portion 34 .
[0107] In the hollow portion 10 , the non-skin side surface ULb of the upper layer UL is a surface that directly contacts the excrement accumulated in the hollow portion 10 .
[0108] Among them, since the diaper has a structure to prevent leakage, the inside of the diaper becomes a hot and humid environment due to moisture such as sweat and urine. Thus, the skin inside the diaper becomes hot and swells, and the barrier function of the skin is easily reduced. In addition, after urination and defecation, the inside of the diaper becomes an environment that easily breeds bacteria.
[0109] In addition, stool contains enzymes such as protease and lipolytic enzymes, and intestinal bacteria such as Escherichia coli and Staphylococcus aureus. Staphylococcus aureus is a harmful bacterium that has an adverse effect on the skin. In diapers, due to urination, urea contained in urine is decomposed by Staphylococcus aureus and converted into ammonia, which easily forms an alkaline environment. When the diaper becomes an alkaline environment, the action of Staphylococcus aureus becomes active, and Staphylococcus aureus produces toxins, causing skin problems such as inflammation, eczema, or skin rashes. In addition, when there is stool in the diaper, the diaper becomes an alkaline environment, so that the action of the enzymes in the stool is activated, which irritates the softened skin and the reduced skin barrier function, and is likely to cause skin problems.
[0110] In contrast, in the diaper 1 using the surface material 2 of the present embodiment, by containing metal oxide antimicrobial agent compounded fibers on the skin side 2a (skin side ULa of the upper layer UL) of the surface material 2 in contact with the wearer's skin, an antimicrobial effect can be exerted from the early stage of excretion.
[0111] Furthermore, in the surface material 2, as described above, the concavoconvex structure including the hollow convex portion 33 is provided, and the skin side ULa and the non-skin side ULb of the upper layer UL that are in direct contact with the excrement of the hollow portion 10 and the concave portion 34 where the excrement is easily retained are configured to contain metal oxide antimicrobial agent compounded fibers in which the metal oxide antimicrobial agent is mixed so as to be easily retained in the surface material 2. Thus, the excrement retained in the hollow portion 10 and the concave portion 34 and the metal oxide antimicrobial agent can be effectively contacted at a high frequency.
[0112] Therefore, even a small amount of the metal oxide antimicrobial agent can effectively and efficiently exert an antimicrobial effect, and can inhibit the growth of bacteria caused by the excrement from the wearer from the early stage of excretion, thereby inhibiting skin problems.
[0113] In addition, since the surface material 2 is provided with the compressed area 52a, the antibacterial effect of the recess 34 can be more effectively and efficiently exhibited. That is, as described above, the compressed area 52a constituting a part of the recess 34 and its vicinity are easily introduced due to the difference in fiber density with the surrounding thereof, and the liquid excreta is not easy to penetrate the compressed area 52a and its vicinity, and the excreta is easily retained in the recess 34. Therefore, the metal oxide antimicrobial agent and the excreta can be effectively contacted.
[0114] In addition, in the pressed area 52a formed by the pressing process accompanied by the melting of the fiber material, the fiber form originally possessed by the surface material sometimes disappears and becomes a membrane. The excreta liquid is less likely to pass through the pressed area 52a in such a membrane state, and the excreta can be more easily retained in the concave portion 34, so that the metal oxide antibacterial agent and the excreta can contact more effectively.
[0115] Thus, in the surface material 2 of the present embodiment, the concavo-convex structure having a hollow portion is provided to form a form in which excrement is easily retained on the surface material, and the metal oxide antimicrobial agent is mixed with the surface material in such a manner that the excrement and the metal oxide antimicrobial agent are in contact with each other at a high frequency in the portion where the excrement is retained. Thus, the antimicrobial effect can be effectively exhibited, and an excellent antimicrobial effect can be obtained with a small content of the metal oxide antimicrobial agent.
[0116] In addition, in the surface material 2, an effective antibacterial effect can be exhibited without mixing the metal oxide antibacterial agent throughout all the layers constituting the surface material, so the content of the metal oxide antibacterial agent can be suppressed to a low level.
[0117] Among them, metal oxide antimicrobial agents act not only on bacteria derived from excrement that cause skin rashes, but also on skin resident bacteria that contribute to the barrier function of the skin, and there is a possibility that the balance of skin resident bacteria will be unbalanced and skin problems may be caused.
[0118] However, in the surface material 2 of this embodiment, a sufficient antibacterial effect can be obtained and the content of the metal oxide antibacterial agent can be suppressed to a low level, so the resident bacteria of the skin will not be unbalanced due to the excessive amount of the metal oxide antibacterial agent, and skin problems can be effectively suppressed and costs can be reduced.
[0119] [About the upper level]
[0120] In the surface material 2 of the present embodiment, as described above, the upper layer UL has a multilayer structure composed of two layers, the first layer 21 and the second layer 22 .
[0121] In addition, the upper layer UL may be composed of one layer or a multilayer structure of three or more layers. In the case of a multilayer structure, the layer constituting the skin side ULa and the layer constituting the non-skin side ULb of the upper layer UL may be respectively constituted to contain metal oxide antibacterial agent compounding fiber. Thus, the skin side ULa and the non-skin side ULb become a form containing metal oxide antibacterial agent compounding fiber.
[0122] In the surface material 2, the content ratio of the metal oxide antibacterial agent in the first layer 21 and the second layer 22 can be the same. From the perspective of obtaining a sufficient antibacterial effect brought by the metal oxide antibacterial agent and reducing the overall amount of the metal oxide antibacterial agent in the surface material 2, it is easier to maintain a good balance of resident bacteria in the skin. Preferably, the content ratio of the metal oxide antibacterial agent in the first layer 21 is higher than that in the second layer 22.
[0123] The first layer 21 is a surface that can directly contact the wearer's skin. The skin side 2a of the surface material 2 formed by the first layer 21 has a concavo-convex structure, which can reduce the contact area between the skin and the surface material 2 and suppress the friction of the skin caused by the surface material 2. On the other hand, by forming the concavo-convex structure, the contact opportunity between bacteria from excrement attached to the skin and the metal oxide antibacterial agent is easily reduced.
[0124] In this regard, in the surface material 2 of the present embodiment, in the upper layer UL, by making the content ratio of the metal oxide antibacterial agent in the first layer 21 relatively high, even with a concavo-convex structure, it is possible to fully ensure the contact opportunity between bacteria from excrement and the metal oxide antibacterial agent, and to obtain a sufficient antibacterial effect. On the other hand, in the second layer 22, the metal oxide antibacterial agent can be added to a sufficient degree of antibacterial effect on the excrement present in the hollow part 10, and the content ratio of the metal oxide antibacterial agent can be relatively lower than that of the first layer 21.
[0125] In this way, in the surface material 2, by making the content ratio of the metal oxide antibacterial agent in the first layer 21 higher than that in the second layer 22, while obtaining a sufficient antibacterial effect brought by the metal oxide antibacterial agent, the overall amount of the metal oxide antibacterial agent in the surface material 2 is reduced, making it easy to maintain a good balance of the resident bacteria in the skin.
[0126] In the surface material 2 of the present embodiment, by forming the upper layer UL with a multilayer structure, the content ratio of the metal oxide antimicrobial agent contained in each of the skin-side side ULa and the non-skin-side side ULb of the upper layer UL can be easily adjusted.
[0127] That is, when the upper layer UL is formed of a multi-layer structure, the content ratio of the metal oxide antibacterial agent in the layer forming the skin side ULa and the layer forming the non-skin side ULb of the upper layer UL is made different, thereby making it easy to adjust the content ratio of the metal oxide antibacterial agent contained in the skin side ULa and the non-skin side ULb of the upper layer UL. As a result, it is easy to adjust the distribution of the metal oxide antibacterial agent in the surface material 2, so that the overall amount of the metal oxide antibacterial agent in the surface material 2 can be reduced and a sufficient antibacterial effect can be obtained.
[0128] [About the lower layer]
[0129] As described above, the lower layer LL (third layer 23) may or may not contain the metal oxide antimicrobial agent compounded fiber.
[0130] In the surface material 2 of the present embodiment, the lower layer LL is a single-layer structure, or a multilayer structure formed by stacking two or more layers. In the case of a multilayer structure, the lower layer LL is configured to include a third layer 23 constituting the skin side LLa. The third layer may contain a metal oxide antibacterial agent compounding fiber, or may not contain a metal oxide antibacterial agent compounding fiber.
[0131] [Relationship between the content ratios of the metal oxide antimicrobial agent in the first layer, the second layer, and the third layer]
[0132] The content ratio of the metal oxide antimicrobial agent in the first layer 21 may be higher than that in the second layer 22 , and the content ratio of the metal oxide antimicrobial agent in the second layer 22 may be higher than that in the third layer 23 .
[0133] In other words, in the surface material 2, the content ratio of the metal oxide antimicrobial agent in the third layer 23 closest to the non-skin side among the three layers (the first layer 21, the second layer 22, and the third layer 23) constituting the surface material 2 can be made the lowest.
[0134] In the surface material 2 of this embodiment, the content of the metal oxide antibacterial agent in the first layer 21 is the highest, the content of the metal oxide antibacterial agent in the second layer 22 is the second, and the content of the metal oxide antibacterial agent in the third layer 23 is the lowest.
[0135] By adopting such a configuration, an effective and efficient antibacterial effect can be obtained, and by reducing the content of the metal oxide antibacterial agent in the entire surface material 2, it is easy to maintain a good balance of the resident bacteria in the skin.
[0136] That is, in the surface material 2, by including the metal oxide antibacterial agent in the skin side ULa and the non-skin side ULb of the upper layer UL, the excrement retained in the hollow portion 10 formed by the non-skin side ULb of the upper layer UL and the recess 34 formed by the skin side ULa can come into contact with the metal oxide antibacterial agent at a high frequency. Therefore, in the surface material 2, even if the content ratio of the metal oxide antibacterial agent in the third layer 23 is relatively low, a sufficient antibacterial effect can be obtained. Therefore, by reducing the content ratio of the metal oxide antibacterial agent in the third layer 23, the amount of the metal oxide antibacterial agent in the surface material 2 as a whole can be reduced, and it is easy to maintain a good balance of the resident bacteria in the skin.
[0137] In the surface material 2 of the present embodiment, from the viewpoint of effectively and efficiently exerting the effect of preventing skin problems brought about by the metal oxide antibacterial agent 6 and better maintaining the balance of resident bacteria in the skin and inhibiting skin problems, the preferred content ratio of the metal oxide antibacterial agent in each of the first layer 21, the second layer and the third layer 23 is as follows. The calculation method of the content ratio of the metal oxide antibacterial agent in each layer will be described later.
[0138] In the first layer 21, the content of the metal oxide antibacterial agent is preferably 0.04 mass % or more and 2.5 mass % or less, and more preferably 0.05 mass % or more and 2.0 mass % or less.
[0139] In the second layer 22, the content of the metal oxide antibacterial agent is preferably 0.025 mass % or more and 2.25 mass % or less, and more preferably 0.045 mass % or more and 1.25 mass % or less.
[0140] In the third layer 23, the content of the metal oxide antibacterial agent is preferably 0 mass % or more and 1.25 mass % or less, and more preferably 0.01 mass % or more and 1.25 mass % or less.
[0141] [Content ratio of metal oxide antimicrobial agent compounding fiber in each of the first layer, the second layer and the third layer]
[0142] For example, by adjusting the content ratio of the metal oxide antibacterial agent in each layer, the content ratio of the metal oxide antibacterial agent in the first layer 21, the second layer 22 and the third layer 23 can be adjusted to satisfy the above-mentioned relationship between the content ratio of the metal oxide antibacterial agent in the first layer, the second layer and the third layer.
[0143] In the surface material 2 of the present embodiment, the preferred content ratio of the metal oxide antimicrobial agent compounded fiber in each of the first layer 21, the second layer 22, and the third layer 23 is as follows.
[0144] In the first layer 21, from the viewpoint of effectively and efficiently performing antibacterial properties on the skin side 2a, the ratio (content ratio) of the metal oxide antibacterial agent compounding fiber in the fibers constituting the first layer 21 is preferably 80 to 100% by mass. In addition, in the present embodiment, the content ratio of the metal oxide antibacterial agent compounding fiber in the first layer 21 is 100% by mass.
[0145] In the second layer 22, from the viewpoint of effectively and efficiently showing antibacterial properties in the hollow portion 10 and maintaining a good balance of resident bacteria in the skin, the ratio (content ratio) of the metal oxide antibacterial agent compounding fiber in the fibers constituting the second layer 22 is preferably 50 to 90% by mass. In addition, in the present embodiment, the content ratio of the metal oxide antibacterial agent compounding fiber in the second layer 22 is 85% by mass.
[0146] In the third layer 23, from the viewpoint of maintaining a good balance of resident bacteria in the skin, the ratio (content ratio) of the metal oxide antimicrobial agent compounding fiber in the fibers constituting the third layer 23 is preferably 0 to 50% by mass. In addition, in the present embodiment, the content ratio of the metal oxide antimicrobial agent compounding fiber in the third layer 23 is 0% by mass.
[0147] [Proportion of metal oxide antimicrobial agent in the total surface material]
[0148] From the perspective of effectively and efficiently exerting the effect of the metal oxide antibacterial agent 6 in preventing skin problems, and better maintaining the balance of resident bacteria in the skin, thereby inhibiting skin problems, the proportion (content ratio) of the metal oxide antibacterial agent in the overall surface material is preferably not less than 0.015 mass % and not more than 2.0 mass %, and more preferably not less than 0.04 mass % and not more than 0.75 mass %.
[0149] The method for calculating the ratio of the metal oxide antimicrobial agent to the entire surface material will be described later.
[0150] [Proportion of metal oxide antimicrobial agent compounded fiber in the total surface material]
[0151] For example, by adjusting the ratio (content ratio) of the metal oxide antimicrobial agent compounded fiber in the entire surface material, the range of the ratio of the metal oxide antimicrobial agent in the entire surface material can be achieved.
[0152] From the perspective of effectively and efficiently exerting the effect of the metal oxide antibacterial agent 6 in preventing skin problems, and better maintaining the balance of resident bacteria in the skin and inhibiting skin problems, the proportion of the metal oxide antibacterial agent combined fiber in the overall surface material is preferably not less than 30 mass % and not more than 80 mass %, and more preferably not less than 40 mass % and not more than 70 mass %.
[0153] [Distance between fibers]
[0154] The fiber density of each of the first layer 21, the second layer 22, and the third layer 23 may be different. In other words, the inter-fiber distance (the gap between fibers) of the first layer 21, the second layer 22, and the third layer 23 may be different from each other.
[0155] "Different fiber densities" means different distances between fibers. "High fiber density" means a state where the distance between fibers is relatively small, and "low fiber density" means a state where the distance between fibers is relatively large. A state where the distance between fibers is small is a state where the fibers are densely packed. When the distance between fibers is small, the attraction of the liquid generated by the capillary becomes larger than when the distance between fibers is large.
[0156] From the viewpoint of more efficiently exerting the antibacterial effect brought about by the metal oxide antibacterial agent, in the surface material 2, the distance between fibers of the first layer 21 is preferably smaller than that of the second layer 22, and the distance between fibers of the second layer 22 is relatively smaller than that of the third layer 23. That is, with respect to the fiber density, the first layer 21 is preferably the highest, the second layer 22 is the second, and the third layer 23 is the lowest.
[0157] By adopting such a configuration, in the thickness direction Z of the surface material 2, excrement can be easily retained at a position close to the skin side ULa of the surface material 2. Thus, the first metal oxide antimicrobial agent compounded fiber 61 and the second metal oxide antimicrobial agent compounded fiber 621 at a position close to the skin side ULa can be effectively brought into contact with excrement at a high frequency.
[0158] In more detail, by forming the above-mentioned structure, in the surface material 2, the first layer 21 has the largest attraction force for the liquid, the second layer 22 has the second largest attraction force, and the third layer 23 has the smallest attraction force. The attraction force of the liquid through the first layer 21 is the largest, and the time for the excrement to remain in the recess 34 can be more reliably ensured. As a result, the contact frequency between the metal oxide antibacterial agent and the excrement can be increased, and antibacterial effect can be effectively achieved. In addition, the excrement that moves to the hollow part 10 through the upper layer UL can more reliably ensure the time for the excrement to temporarily remain in the hollow part 10 by utilizing the difference in the attraction force of the liquid generated by the difference in the distance between the fibers of the second layer 22 and the third layer 23. As a result, the contact frequency between the excrement in the hollow part 10 and the metal oxide antibacterial agent can be increased, and antibacterial effect can be effectively achieved.
[0159] The adjustment of the distance between fibers of each layer can be performed by making the fiber diameters of the fibers used in each layer different. As an example, in the surface material 2 of the present embodiment, the fiber diameters of the first metal oxide antimicrobial agent compounding fiber 61 and the second metal oxide antimicrobial agent compounding fiber 621 are 15 μm, and the fiber diameters of the second metal oxide antimicrobial agent non-combining fiber 622 and the third metal oxide antimicrobial agent non-combining fiber 63 are 20 μm, thereby enabling the distance between fibers of the first layer 21, the second layer 22, and the third layer 23 to be in the above-mentioned relationship.
[0160] Furthermore, when the upper layer UL and the lower layer LL are each composed of one layer, in the surface material, it is preferred that the distance between fibers of the upper layer UL is relatively smaller than that of the lower layer LL.
[0161] By adopting such a configuration, in the surface material 2, the attraction force of the liquid is the largest in the upper layer UL and the smallest in the lower layer LL. Since the attraction force of the liquid is the largest in the upper layer UL, the time for the excrement to remain in the concave portion 34 can be more reliably ensured, and the contact frequency between the metal oxide antibacterial agent and the excrement can be made higher, thereby achieving effective antibacterial effect. In addition, the excrement that moves to the hollow portion 10 through the upper layer UL can more reliably ensure the time for the excrement to temporarily remain in the hollow portion 10 due to the difference in the distance between the fibers of the upper layer UL and the lower layer LL, thereby achieving effective antibacterial effect.
[0162] Specific numerical values of the distances between fibers of each of the first layer 21 , the second layer 22 , and the third layer 23 are listed below, but these are merely examples and the present invention is not limited to these.
[0163] In the surface material 2, from the viewpoint of more reliably ensuring the time that excrement remains in the recess 34 and increasing the contact frequency between the metal oxide antibacterial agent and the excrement, the distance between fibers of the first layer 21 is preferably greater than 30 μm, more preferably greater than 50 μm, preferably less than 100 μm, more preferably less than 80 μm, preferably greater than 30 μm and less than 100 μm, more preferably greater than 50 μm and less than 80 μm.
[0164] From the viewpoint that the excrement moved to the hollow portion 10 is more easily temporarily retained in the hollow portion 10 and the contact frequency between the metal oxide antibacterial agent and the excrement is increased, the difference between the fiber distance of the second layer 22 and the fiber distance of the third layer 23 is preferably greater than 10 μm, and more preferably greater than 20 μm.
[0165] The inter-fiber distance of the second layer 22 is preferably 40 μm or more, more preferably 60 μm or more, preferably 110 μm or less, more preferably 90 μm or less, preferably 40 μm or more and 110 μm or less, more preferably 60 μm or more and 90 μm or less.
[0166] The value of the distance between fibers of the third layer 23 is preferably 50 μm or more, more preferably 70 μm or more, preferably 190 μm or less, more preferably 170 μm or less, preferably 50 μm or more and 190 μm or less, more preferably 70 μm or more and 170 μm or less.
[0167] The method for measuring the distance between fibers will be described later.
[0168] [Solubility of Metal Oxide Antimicrobial Agents]
[0169] From the perspective of making the effect of preventing skin rash (skin problems) caused by stool more significant for a long time, the metal oxide antibacterial agent mixed in the metal oxide antibacterial agent compounding fiber is preferably poorly soluble in water. The solubility in water can be evaluated by the solubility obtained by the solubility determination method described below.
[0170] The solubility of the metal oxide antibacterial agent is preferably 0.01 g / 100 ml to 0.5 g / 100 ml, more preferably 0.03 g / 100 ml to 0.3 g / 100 ml, and even more preferably 0.05 g / 100 ml to 0.2 g / 100 ml.
[0171] <Example of method for producing surface material>
[0172] An example of a method for producing the surface material 2 is given below, but the present invention is not limited thereto.
[0173] The surface material 2 having a concave-convex surface on the skin side 2a and a flat surface on the non-skin side 2b can be manufactured as follows: a nonwoven fabric composed of a first metal oxide antimicrobial agent compounded fiber 61, a nonwoven fabric composed of a laminate of a second metal oxide antimicrobial agent compounded fiber 621 and a second metal oxide antimicrobial agent non-compounded fiber 622, and a nonwoven fabric composed of a third metal oxide antimicrobial agent non-compounded fiber 63 are overlapped, and these nonwoven fabrics are partially joined.
[0174] The upper layer UL of the surface material 2 is formed by a laminate of the nonwoven fabric composed of the first metal oxide antimicrobial agent compounded fiber 61 and a laminate of the second metal oxide antimicrobial agent compounded fiber 621 and the second metal oxide antimicrobial agent non-compounded fiber 622 .
[0175] The nonwoven fabric composed of the third metal oxide antimicrobial agent non-compounded fibers 63 constitutes the lower layer LL of the surface material 2 .
[0176] As an example of the production method, the production method described in Japanese Patent Application Laid-Open No. 2004-174234 can be used.
[0177] That is, by biting a sheet of nonwoven fabric constituting the upper layer UL between two gear rollers meshing with each other and having a concave-convex shape on the circumferential surface, the sheet is intermittently stretched to perform a concave-convex shaping process. In this way, in the sheet after the concave-convex processing, the stretched part constitutes the convex part 33. On the other hand, the part that is not stretched constitutes the concave part 34 when the surface material 2 is made. In this way, the sheet constituting the upper layer UL formed with a plurality of convex parts 33 is overlapped with the sheet constituting the lower layer LL, and the overlap is clamped between two rollers at least one of which is heated to a specified temperature for partial bonding. As a result, the upper layer UL and the lower layer LL are pressed, and are partially bonded by heat fusion in the pressing area 52a (a part of the concave part 34), so as to manufacture a surface material 2 with a concave-convex structure. The surface on the upper layer UL side (skin side 2a) of the surface material 2 has concave-convex, and the surface on the lower layer LL side (non-skin side 2b) of the surface material 2 is roughly flat.
[0178] <Supplementary explanation>
[0179] [Method for confirming hollow convex parts, etc.]
[0180] Whether the surface material has projections and depressions and the projections have hollow parts can be confirmed by cutting the surface material with a razor (for example, a single-edged razor manufactured by Feather Safety Razor Co., Ltd.) to obtain a measurement piece, and then magnifying and observing the cut surface of the measurement piece.
[0181] For example, using a field emission type electron microscope S-4000 manufactured by Hitachi, Ltd., the magnification is adjusted to allow all layers to be included in the field of view, and the cross section of the test piece is observed.
[0182] When observing the cut surface, an object of known size is simultaneously illuminated, so that the size of each component such as the height of the protrusion 33 and the thickness of each layer can be obtained.
[0183] By observing the cut surface, it can be confirmed that the surface material is composed of stacked layers having different inter-fiber distances.
[0184] By observing the cut surface, in addition to understanding the cross-sectional profile of the fiber, it is also possible to grasp the fiber structure such as core-sheath type fiber or single fiber structure. In addition, in the case of core-sheath type fiber, by observing the cut surface, the area ratio of the core and the sheath can be calculated.
[0185] By observing the cut surface, it is possible to confirm the presence of the metal oxide antimicrobial agent in the fiber, the presence of the metal oxide antimicrobial agent in the sheath, and the exposure of the metal oxide antimicrobial agent on the fiber surface.
[0186] In addition, by performing SEM-EDX analysis on the fiber cross section, it was confirmed that the agent contained in the sheath was zinc oxide (metal oxide antibacterial agent).
[0187] [Calculation method of the content ratio of the metal oxide antimicrobial agent in the first layer, the second layer, and the third layer]
[0188] Weigh 1g of the target layer (first layer, second layer or third layer) of the surface material, cut it as small as possible, put it into a 300ml beaker, add 200ml of ion exchange water to the beaker, and stir it with a magnetic stirrer to make the fiber completely contact with water. While stirring the liquid, add 3ml of concentrated hydrochloric acid (about 10M) in small amounts at a time, and stir for another hour to dissolve the metal oxide antibacterial agent present on the surface of the fiber constituting the target layer. Next, add 6ml of 5.1M sodium hydroxide aqueous solution to neutralize the liquid, and then add 10ml of pH 10.7 buffer solution (containing 54.7ml of 28 mass% NH3 aqueous solution and 0.535g of NH4Cl, dissolved in ion exchange water) to fine-tune the pH.
[0189] Next, add chrome black T reagent (0.125g of chrome black T powder and 1.125g of hydroxylamine hydrochloride dissolved in 25ml of anhydrous ethanol) as an indicator to make the liquid pale pink. Use 0.0002M EDTA·2Na as a titrant and titrate. The amount of the titrant added (ml) when the liquid changes from pink to light blue to green is taken as the titration value A. Then, the mass of the metal oxide antibacterial agent is calculated using the following formula. "5000000" in the following formula means the volume (ml) of the titrant per 1mol.
[0190] The mass of metal oxide antibacterial agent (g) = titration value A × the mass of metal oxide antibacterial agent per 1 mol / 5000000
[0191] The mass of the metal oxide antimicrobial agent calculated by the above operation is the mass of the metal oxide antimicrobial agent contained in 1 g of the target layer. Therefore, the value obtained by multiplying the calculated mass of the metal oxide antimicrobial agent by 100 times becomes the content ratio of the metal oxide antimicrobial agent in the target layer.
[0192] [Calculation method of the ratio of metal oxide antimicrobial agent in the entire surface material]
[0193] As the object sample, 1 g of the surface material is weighed in a manner including the first layer, the second layer and the third layer, and the proportion of the metal oxide antibacterial agent in the entire surface material is calculated using the same method as the calculation method of the proportion of the metal oxide antibacterial agent in the first layer, the second layer and the third layer mentioned above.
[0194] [Method for measuring the distance between fibers]
[0195] The inter-fiber distance of a nonwoven fabric as a fiber assembly is calculated using the following formula (1) based on Wrotonowski's assumption. The following formula (1) is usually used when solving the inter-fiber distance of a fiber assembly. Under Wrotonowski's assumption, the fibers are cylindrical, and each fiber does not intersect with each other, but is arranged regularly.
[0196] The surface material to be measured has a multilayer structure including a first layer constituting a sparse region and a second layer constituting a dense region. The inter-fiber distances of the sparse region and the dense region are calculated using the following formula (1).
[0197] In the calculation, the thickness t, gram weight W, fiber resin density ρ, and fiber diameter D used in the following formula (1) use the respective values of the sparse area (first layer) and dense area (second layer) of the measurement object. The thickness t, gram weight W, and fiber diameter D are the average values of the measured values at multiple measurement points.
[0198] The thickness t (mm) is measured by the following method. First, the surface material of the object to be measured is cut into a size of 50 mm in the X direction and 50 mm in the Y direction to make a slice of the surface material. Then, the slice is placed on a flat plate, and a glass plate on the flat plate is placed on it. After weights are evenly placed on the glass plate so that the load including the glass plate becomes 49 Pa, the thickness of the slice is measured. The measurement environment is a temperature of 20±2°C and a relative humidity of 65±5%, and a microscope (manufactured by Keyence Co., Ltd., VHX-1000) is used as the measuring instrument. Regarding the measurement of the thickness of the slice, first, an enlarged photograph of the cut surface of the slice is obtained. An object of known size is simultaneously projected into the enlarged photograph. Next, the scale is aligned with the enlarged photograph of the cut surface of the above-mentioned slice, and the thickness of the sparse area and the dense area of the slice is measured. The above operation is performed 3 times, and the average value of the 3 times is taken as the thickness t of the layer of the object to be measured.
[0199] In the cut surface of the slice, the sparse area and the dense area are distinguished according to the following method. Compared with the dense area, the density of the constituent fibers in the sparse area is lower (the distance between fibers is larger), so in the cut surface of the slice, the area with a relatively large distance between fibers is the sparse area, and the area with a relatively small distance between fibers is the dense area. These two areas can be distinguished even with the naked eye.
[0200] Weight W(g / m 2 ) is obtained by cutting the sparse area and dense area of the surface material of the measured object into a predetermined size (e.g., 12 cm × 6 cm, etc.), measuring the mass, and dividing the mass measurement value by the area obtained according to the predetermined size to obtain the gram weight W ("gram weight W (g / m 2 )=mass÷area calculated from the specified size”). Repeat this measurement 4 times and take the average value as the gram weight.
[0201] The fiber resin density ρ(g / cm 3 ) The density gradient tube was used for measurement based on the density gradient tube method described in JIS L1015 Test Method for Chemical Staple Fibers (URL: http: / / kikakurui.com / l / L1015-2010-01.html, described in JIS Handbook Fibers-2000 (Japan Standards Association) p.764-p.765 as a book).
[0202] The fiber diameter D (μm) was measured using a Hitachi S-4000 field emission scanning electron microscope on 10 fiber cross sections collected from the sparse region and the dense region, and the average value was taken as the fiber diameter D (μm).
[0203] The fiber diameter D is measured in accordance with the [Method for measuring fiber diameter] described later.
[0204]
[0205] D: Fiber diameter (um)
[0206] 0:Fiber resin density (g / cm3)
[0207] t: thickness (mm)
[0208] W: Weight (g / m 2 )
[0209] [Measurement method of fiber diameter]
[0210] The surface material of the measurement object is cut off from an area not including the pressed area using a razor (e.g., a single-edged razor manufactured by Feather Safety Razor Co., Ltd.) to obtain a measurement piece having a quadrilateral shape when viewed from above. When cutting the measurement object, care should be taken that the structure of the cut surface of the measurement piece formed by cutting is not destroyed by the pressure during cutting, etc. As a preferred method for cutting the measurement object, the following method can be cited: before cutting the measurement object, the measurement object is placed in liquid nitrogen to be fully frozen, and then cut.
[0211] The test piece was attached to the sample stage using double-sided paper tape (Nicetack NW-15 manufactured by Nichiban Co., Ltd.) Next, the test piece was coated with platinum. The coating was performed using an ion sputtering device E-1030 (trade name) manufactured by Hitachi Naka Seiki Co., Ltd., and the sputtering time was 30 seconds.
[0212] The cut surface of the test piece was observed at a magnification of 1000 times using a field emission type electron microscope S-4000 manufactured by Hitachi, Ltd.
[0213] The surface material has sparse areas and dense areas. Therefore, the electron microscope image is used to determine the boundary between the sparse areas and the dense areas based on the difference in the distance between the fibers. For 10 fibers existing in each layer (sparse area or dense area), the length in the width direction relative to the length direction of the fiber is measured respectively, and the average value is taken as the fiber diameter.
[0214] By observing the cut surface of the surface material, it is possible to determine whether the distance between fibers is relatively large or relatively small, and to determine the density of the surface material. Therefore, by observing the cut surface of the surface material, it is possible to confirm that the metal oxide antibacterial agent exists only in the dense area.
[0215] [Method for Determining the Solubility of Metal Oxide Antimicrobial Agents]
[0216] 5 g of the metal oxide antibacterial agent was added to 100 ml of water and stirred at 300 rpm for 30 minutes at room temperature (25° C.) In addition, the mass of the filter paper was measured and the measured mass was taken as the initial mass of the filter paper.
[0217] The stirred solution was filtered using the measured mass of the filter paper, and the filter paper was dried at 40° C. for 2 hours using a dryer. The mass of the dried filter paper was measured, and the measured mass was taken as the mass of the dried filter paper. Then, the solubility was calculated using the following formula.
[0218] Solubility (g) = 5 (g) - {(mass of filter paper after drying) (g) - (initial mass of filter paper) (g)}
[0219] The larger the solubility calculated in this way, the greater the solubility in water, and the smaller the solubility, the lower the solubility in water.
[0220] <Other embodiments>
[0221] As mentioned above, although embodiment of this invention was described, this invention is not limited to the said embodiment, It is a matter of course that various changes can be made within the range which does not deviate from the summary of this invention.
[0222] For example, in the above embodiments, disposable diapers are exemplified as absorbent articles, but the present invention is not limited thereto. The absorbent articles of the present invention may be urine-absorbing pads, sanitary pads, sanitary napkins, etc., and the surface material of these absorbent articles may be the surface material of the present invention. Absorbent articles are generally composed of a liquid-permeable surface material, a liquid-impermeable back material, and a liquid-retaining absorbent body disposed between the two sheets.
[0223] In each of the above-mentioned embodiments, the metal oxide antimicrobial agent-blended fiber may contain an antimicrobial agent such as a surfactant or an organic compound other than the metal oxide antimicrobial agent.
[0224] In addition, the metal oxide antimicrobial agent compounded fiber may contain a skin care agent.
[0225] As the skin conditioning agent, a hydrophobic skin conditioning agent, a hydrophilic skin conditioning agent, and the like can be used.
[0226] A hydrophobic skin care agent is a hydrophobic component that is not water-soluble and water-dispersible, or has extremely low solubility, and is a composition or compound that has effects such as protecting and healing the skin of the wearer. More specifically, a hydrophobic component refers to a component that dissolves less than 1 g when 10 g of a preparation of the component is mixed in 1 L of ion-exchanged water and left to stand for 24 hours, preferably a component that dissolves less than 0.1 g, and particularly preferably a component that does not dissolve at all.
[0227] As hydrophobic skin care agents, fatty acids with carbon chain lengths of 12 to 28 or ester compounds of the fatty acids and glycerol, waxes, vaseline, etc. can be cited, and unsaturated fatty acids with carbon chain lengths of 12 to 28 or glyceride compounds of the unsaturated fatty acids are particularly preferred. The glyceride is a monoester, diester or triester of glycerol and the above-mentioned unsaturated fatty acids, and triesters are particularly preferred. As preparations containing fatty acids or fatty acid compounds, it is preferred to use natural extracts such as argan oil and shea butter. In particular, argan oil, which is a hydrophobic plant oil containing unsaturated fatty acids, maintains the balance of moisture and oil in the skin, prevents dryness, and functions as a skin care agent. In addition, argan oil contains many unsaturated fatty acids such as oleic acid and linoleic acid, and has a strong ability to remove active oxygen, for example, it can reduce skin damage caused by sun exposure.
[0228] On the other hand, a hydrophilic skin care agent is a water-soluble or water-dispersible hydrophilic component, preferably a component that can inhibit the occurrence of rash or inflammation, and when rash or inflammation occurs, inhibit the progression of the rash or inflammation, or relieve the rash or inflammation. More specifically, a hydrophilic component refers to a component that dissolves or disperses in an amount of 1 g or more, preferably 5 g or more, more preferably 1 g or more, and even more preferably 5 g or more, and most preferably completely dissolved, when 10 g of a preparation of the component is mixed in 1 L of ion exchange water and left to stand for 24 hours.
[0229] As the hydrophilic skin care agent, there can be used natural extracts such as peach leaf extract and witch hazel extract, polyols having 2 to 4 carbon atoms, polyethylene glycol, and hydrophilic compounds having skin care functions.
[0230] Among these, peach leaf extract (hydrophilic extract) as a plant extract has antibacterial action and anti-inflammatory action and is preferred. Peach leaf extract as a hydrophilic component dissolves in the liquid supplied to the surface material and transfers to the skin, thereby producing a skin care effect.
[0231] Polyols with 2 to 4 carbon atoms are hydrophilic components, typically 1,3-butylene glycol. By using 1,3-butylene glycol, moisturizing effect and lubricity are improved. By improving lubricity, friction between skin and nonwoven fabric can be reduced, and skin damage can be suppressed. 1,3-butylene glycol is a liquid water-soluble base component with moisturizing properties, has a smooth feel, and has a low stickiness, keeping the skin moisturized. In addition to being used as a moisturizer, 1,3-butylene glycol can also be used as a solvent. For example, when peach leaf extract is used as a skin care agent, 1,3-butylene glycol can be used as a solvent for peach leaf extract. In addition, 1,3-butylene glycol is cited as an example here, but as long as it is a polyol with 2 to 4 carbon atoms, it can show the same effect, for example, propylene glycol can also be used. Propylene glycol can also be used as an extraction solvent for peach leaf extract (hydrophilic extract).
[0232] The present invention may also adopt the following configurations.
[0233] <1> A surface material of an absorbent article, the surface material having a skin side and a non-skin side, the skin side having a plurality of convex portions and a plurality of concave portions between the plurality of convex portions,
[0234] The surface material of the absorbent article comprises an upper layer constituting the skin side and a lower layer constituting the non-skin side.
[0235] The convex portion has a hollow portion therein, and the hollow portion is located between the upper layer and the lower layer.
[0236] The fibers constituting the non-skin side of the upper layer forming the hollow portion and the fibers constituting the skin side of the upper layer include metal oxide antimicrobial agent-blended fibers, and the metal oxide antimicrobial agent-blended fibers are fibers containing a metal oxide antimicrobial agent.
[0237] <2> The surface material of the absorbent article according to <1> above, wherein the metal oxide antimicrobial agent-compounded fiber is obtained by mixing the metal oxide antimicrobial agent into fibers.
[0238] <3> The surface material of the absorbent article according to <1> or <2> above, wherein the upper layer includes a first layer constituting the skin-side surface and a second layer constituting the non-skin-side surface.
[0239] <4> The surface material for an absorbent article according to <3> above, wherein the content of the metal oxide antimicrobial agent in the second layer is lower than that in the first layer.
[0240] <5> The surface material of the absorbent article according to <4> above, wherein the lower layer includes a third layer constituting the skin side of the lower layer,
[0241] The content of the metal oxide antimicrobial agent in the third layer is lower than that in the second layer.
[0242] <6> The surface material of the absorbent article according to <5> above, wherein the content ratio of the metal oxide antimicrobial agent compounding fiber relative to the mass of each of the first layer, the second layer and the third layer is
[0243] In the first layer, it is 80% by mass or more and 100% by mass or less,
[0244] In the second layer, it is 50% by mass or more and 90% by mass or less,
[0245] In the third layer, the content is 0 mass % or more and 50 mass % or less.
[0246] <7> The surface material of the absorbent article according to <5> above, wherein the content ratio of the metal oxide antimicrobial agent relative to the mass of each of the first layer, the second layer and the third layer is
[0247] In the first layer, the content is preferably 0.04 mass % to 2.5 mass %, more preferably 0.05 mass % to 2.0 mass %.
[0248] In the second layer, the content is preferably 0.025 mass % to 2.25 mass %, more preferably 0.045 mass % to 1.25 mass %.
[0249] In the third layer, the content is preferably 0 mass % to 1.25 mass %, and more preferably 0.01 mass % to 1.25 mass %.
[0250] <8> The surface material of the absorbent article as described in any one of <5> to <7> above, wherein the distance between fibers of the first layer is smaller than the distance between fibers of the second layer, and the distance between fibers of the second layer is smaller than the distance between fibers of the third layer.
[0251] <9> The surface material of the absorbent article according to <8> above, wherein the distance between the fibers of the first layer is preferably from 30 μm to 100 μm, more preferably from 50 μm to 80 μm,
[0252] The distance between the fibers of the second layer is preferably 40 μm to 110 μm, more preferably 60 μm to 90 μm.
[0253] The distance between fibers in the third layer is preferably from 50 μm to 190 μm, and more preferably from 70 μm to 170 μm.
[0254] <10> The surface material for an absorbent article according to <8> or <9>, wherein the difference between the distance between fibers of the second layer and the distance between fibers of the third layer is preferably 10 μm or more, more preferably 20 μm or more.
[0255] <11> A surface material for an absorbent article as described in any one of <1> to <10> above, wherein the metal oxide antimicrobial agent compounded fiber is a core-sheath type fiber having a core portion and a sheath portion, the metal oxide antimicrobial agent is compounded in the sheath portion, and the metal oxide antimicrobial agent is exposed on the surface of the metal oxide antimicrobial agent compounded fiber.
[0256] <12> The surface material of the absorbent article according to <11> above, wherein the ratio of the metal oxide antimicrobial agent in the core-sheath type fiber is 0.05 mass % or more and 2.5 mass % or less.
[0257] <13> The surface material for an absorbent article according to any one of <1> to <12>, wherein the metal oxide antimicrobial agent is zinc oxide.
[0258] <14> The surface material for an absorbent article according to any one of <1> to <13>, wherein the ratio of the metal oxide antimicrobial agent-blended fiber to the entire surface material is 30% by mass or more and 80% by mass or less.
[0259] <15> The surface material for an absorbent article according to any one of <1> to <13>, wherein the ratio of the metal oxide antimicrobial agent to the entire surface material is 0.015% by mass or more and 2.0% by mass or less.
[0260] <16> The surface material for an absorbent article according to any one of <1> to <15>, wherein the recessed portion is formed by partially pressing the upper layer and the lower layer.
[0261] <17> An absorbent article comprising:
[0262] an absorber; and
[0263] The surface material according to any one of <1> to <16> above, which is located on the skin-side surface of the absorbent body.
[0264] Industrial Applicability
[0265] The surface material of the absorbent article of the present invention can exhibit an effective antibacterial effect.
Claims
1. A surface material for an absorbent article, characterized in that: It has a skin side and a non-skin side, wherein the skin side has a plurality of convex portions and a plurality of concave portions between the plurality of convex portions. The surface material of the absorbent article has an upper layer constituting the skin side and a lower layer constituting the non-skin side. The convex portion has a hollow portion inside thereof, and the hollow portion is located between the upper layer and the lower layer. The fibers constituting the non-skin side of the upper layer and the fibers constituting the skin side of the upper layer forming the hollow portion include metal oxide antimicrobial agent-blended fibers, which are fibers containing a metal oxide antimicrobial agent.
2. The surface material of the absorbent article according to claim 1, characterized in that: The metal oxide antimicrobial agent compounded fiber is obtained by mixing the metal oxide antimicrobial agent into the fiber.
3. The surface material of the absorbent article according to claim 1 or 2, characterized in that: The upper layer includes a first layer constituting the skin side and a second layer constituting the non-skin side.
4. The surface material of the absorbent article according to claim 3, characterized in that: The content ratio of the metal oxide antimicrobial agent in the second layer is lower than that in the first layer.
5. The surface material of the absorbent article according to claim 4, characterized in that: The lower layer comprises a third layer constituting the skin side of the lower layer, The content ratio of the metal oxide antimicrobial agent in the third layer is lower than that in the second layer.
6. The surface material of the absorbent article according to claim 5, characterized in that: The content ratio of the metal oxide antimicrobial agent compounding fiber relative to the mass of each of the first layer, the second layer and the third layer, In the first layer, the content is 80% by mass or more and 100% by mass or less, In the second layer, it is 50 mass % or more and 90 mass % or less, In the third layer, the content is 0 mass % or more and 50 mass % or less.
7. The surface material of the absorbent article according to claim 5, characterized in that: The content ratio of the metal oxide antibacterial agent relative to the mass of each of the first layer, the second layer and the third layer, In the first layer, the content is 0.04 mass % or more and 2.5 mass % or less, In the second layer, the content is 0.025 mass % or more and 2.25 mass % or less, In the third layer, the content is 0 mass % or more and 1.25 mass % or less.
8. The surface material of the absorbent article according to any one of claims 5 to 7, characterized in that: The distance between fibers of the first layer is smaller than the distance between fibers of the second layer, and the distance between fibers of the second layer is smaller than the distance between fibers of the third layer.
9. The surface material of the absorbent article according to claim 8, characterized in that: The distance between the fibers of the first layer is not less than 30 μm and not more than 100 μm, The distance between the fibers of the second layer is not less than 40 μm and not more than 110 μm, The distance between fibers in the third layer is not less than 50 μm and not more than 190 μm.
10. The surface material of the absorbent article according to claim 8 or 9, characterized in that: A difference between a distance between fibers of the second layer and a distance between fibers of the third layer is 10 μm or more.
11. The surface material of the absorbent article according to any one of claims 1 to 10, characterized in that: The metal oxide antimicrobial agent compounded fiber is a core-sheath type fiber having a core portion and a sheath portion. The metal oxide antimicrobial agent is compounded in the sheath portion and the metal oxide antimicrobial agent is exposed on the surface of the metal oxide antimicrobial agent compounded fiber.
12. The surface material of the absorbent article according to claim 11, characterized in that: The ratio of the metal oxide antimicrobial agent in the core-sheath type fiber is 0.05 mass % or more and 2.5 mass % or less.
13. The surface material of the absorbent article according to any one of claims 1 to 12, characterized in that: The metal oxide antibacterial agent is zinc oxide.
14. The surface material of the absorbent article according to any one of claims 1 to 13, characterized in that: The ratio of the metal oxide antimicrobial agent compounded fiber to the entire surface material is 30 mass % or more and 80 mass % or less.
15. The surface material of the absorbent article according to any one of claims 1 to 13, characterized in that: The ratio of the metal oxide antimicrobial agent to the entire surface material is 0.015 mass % or more and 2.0 mass % or less.
16. The surface material of the absorbent article according to any one of claims 1 to 15, characterized in that: The recessed portion is formed by partially pressing the upper layer and the lower layer.
17. An absorbent article, characterized in that: have: an absorber; and The surface material according to any one of claims 1 to 16, which is located on the skin-side surface of the absorbent body.