Multifunctional metal-active protein coating and preparation method thereof
Through the chemical modification of aqueous silane coupling agents with polyphenols and hyaluronic acid, a stable metal-active protein coating is formed, which solves the problem of the stability and stability of metal-protein coatings in biosensors and medical implant materials in the existing technology. safety issues, achieving efficient biofunctionality and antifouling properties.
Patent Information
- Application Number
- CN202410784949.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-22
AI Technical Summary
Existing metal-protein coatings are difficult to meet the requirements for biological safety, biorecognition, transportability and structural stability in the fields of medical implant materials and biosensors, and commonly used preparation methods have problems with toxic side reactions and insufficient stability. .
Water-based silane coupling agents are used to chemically modify materials such as polyphenols and hyaluronic acid to form a multifunctional metal-active protein coating, which fixes proteins and metal ions on the surface of the material through covalent and non-covalent interactions to form a stable Hydration layer to maintain protein activity and anti-fouling properties.
It achieves the construction of stable, safe, broad-spectrum and efficient metal-active protein coatings on biosensors and medical implant materials, improves biological functionality and anti-fouling properties, and avoids protein denaturation and toxic side effects in traditional methods. reaction.
Smart Images

Figure CN118807003A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomaterials, and in particular relates to a multifunctional metal-active protein coating and a preparation method thereof. Background Art
[0002] Surface engineering strategies have been widely studied by changing the physical and chemical properties of the material surface to achieve specific performance and functions. It provides broad possibilities for material design and application, and promotes technological innovation and application development in many fields. Among them, metal-protein coating is a layer of metal-protein complex formed on the surface of materials and devices, which gives the surface metal-protein related properties and functions. It is widely used in biosensors and diagnostic equipment, medical implant materials and devices, etc.
[0003] Depending on the application environment of the metal-protein composite surface, the method or technical means of preparing the coating are also different. Metal-protein coatings used in medical implant materials / devices need to maintain the activity of adsorbed proteins more. According to research, hydrophilic surfaces are more conducive to maintaining the natural conformation of proteins. The more studied hydrophilic surfaces include fixed polyethylene glycol and amphiphilic ion molecular brushes; however, the acquisition of such surfaces not only requires specific elemental components on the grafted surface, but also often involves toxic and harmful substances in the grafting process, which are very likely to cause uncertain toxic and side effects after contact with the body. Moreover, the polyethylene glycol and amphiphilic ion molecular brush surfaces will resist the nonspecific adhesion of proteins, making it difficult to efficiently construct stable and safe metal-active protein coatings. At the same time, in addition to excellent biocompatibility, metal-protein coatings used in biosensors and diagnostic equipment or membrane materials have high requirements for their specificity, biorecognition, transferability and environmental stability. In order to ensure the above functions, the prepared metal-active protein surface must also have excellent anti-fouling and structural stability. However, the currently commonly used methods for preparing metal-protein coatings, such as physical adsorption, spray coating, and sol-gel method, are difficult to meet the above requirements.
[0004] Therefore, based on the above problems, the technical solution of the present invention is proposed. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a multifunctional metal-active protein coating and a preparation method thereof. The preparation method can directly construct a coating on the surface of a substrate material of a biosensor and diagnostic equipment, a medical implant material and an apparatus, and selectively and stably modify the multifunctional metal-active protein coating on the surface according to the service environment and requirements of the substrate material, so that the surface has specific or broad-spectrum biological functions, and better meets the biosafety and biofunctionality of the material or apparatus.
[0006] The solution of the present invention is to provide a method for preparing a multifunctional metal-active protein coating, the preparation method comprising: (1) mixing and dissolving an aqueous silane coupling agent with water to obtain an aqueous silane coupling agent solution; and immersing a substrate material in the aqueous silane coupling agent solution to react to obtain a first reaction sample; (2) dissolving the polyphenol compound and the thiolated hyaluronic acid in an alkaline buffer solution to obtain a polyphenol solution and a hyaluronic acid solution, respectively; (3) immersing the first reaction sample obtained in step (1) in the polyphenol solution for reaction to obtain a second reaction sample; (4) immersing the second reaction sample in the hyaluronic acid solution to react, thereby obtaining a third reaction sample; (5) Dissolving the protein and the metal compound in PBS solution to obtain a protein solution and a metal ion solution, respectively; (6) Mixing equal volumes of the protein solution and the metal ion solution to obtain a mixed solution; and completely immersing the third reaction sample in the mixed solution to react, thereby obtaining a multifunctional metal-active protein coating.
[0007] In order to facilitate understanding of the present invention, the reaction principle of the present invention is explained: The preparation method of the present invention first treats the substrate material with a water-soluble silane coupling agent, generates different chemical groups on the surface of the material, such as silane groups and amine groups / carboxyl groups / methoxy groups, etc., so that the material is converted from an inert surface to an active surface, and the wettability of the material is improved. Subsequently, the activated substrate is placed in a polyphenol compound solution. Under alkaline conditions, the polyphenol undergoes self-oxidation and polymerization reactions on the one hand, generating polyphenol polymers containing quinone groups, carbon-carbon double bonds, etc.; on the other hand, the phenolic hydroxyl groups, amine groups, carboxyl groups, double bonds, etc. of the polyphenol and the polyphenol polymer and the silane groups, amine groups, etc. on the surface of the dialysis material are reacted by silane group and hydroxyl group condensation reaction, silane group and amine group condensation reaction, silane group and carboxyl group esterification reaction and Michael addition, Schiff base, free radical polymerization, hydrogen bonding and other chemical reactions, so that the polyphenol and its polymer are firmly modified on the surface of the substrate material. Subsequently, the thiol group of the hyaluronic acid undergoes a nucleophilic addition reaction with the double bonds of the polyphenol polymer on the surface of the material, and the hyaluronic acid is grafted to the surface, so that the surface obtains excellent wettability. The pre-modified material is immersed in a mixture of protein and metal ions. On the one hand, a large number of active groups on the surface of the coating, including quinone groups, phenolic hydroxyl groups, amine groups, carboxyl groups, benzene rings, etc., can fix the protein to the surface through covalent and non-covalent interactions; on the other hand, the metal ions in the solution react with the phenolic hydroxyl groups and proteins in the coating at the same time. The metal ions, as an "anchor point", not only increase the stability of the entire coating, but also give the coating metal ions corresponding biological functions. It is worth noting that the active functional groups and metal ions on the surface can non-specifically and firmly modify the protein on the surface of the material through covalent and non-covalent interactions, ensuring the broad spectrum and stability of the adsorbed protein; at the same time, hyaluronic acid gives the surface high wettability, so that the hydration layer formed quickly on the surface can maintain the natural conformation of the adsorbed protein, retain the activity and corresponding biological functions of the protein, and also give the coating excellent anti-fouling properties. A stable multifunctional metal-active protein coating was constructed through a clever and efficient method.
[0008] Preferably, the water-based silane coupling agent is one or a combination of two or more of an aminosilane coupling agent, a methylsilane coupling agent, an acrylic silane coupling agent, and an ethoxysilane coupling agent; The aminosilane coupling agent is one or a combination of two or more of aminomethyltriethoxysilane, aminoethyltriethoxysilane, aminoethyltrimethoxysilane, aminopropyltrimethoxysilane, etc. The methylsilane coupling agent is one or a combination of two or more of methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, etc.; The acrylic silane coupling agent is one or a combination of two or more of acrylic trimethoxysilane, acrylic triethoxysilane, acrylic triisopropoxysilane, etc.; The ethoxysilane coupling agent is one or a combination of two or more of ethoxytrimethoxysilane, ethoxytriethoxysilane, ethoxymethyltrimethoxysilane, etc.
[0009] Preferably, the base material is one of a medical metal-based material, a medical ceramic-based material, a medical polymer-based material or a medical composite material.
[0010] Preferably, the alkaline buffer is one of sodium bicarbonate / sodium carbonate buffer, trimethylamine / hydrochloric acid buffer, phosphate buffer, ammonia / ammonium chloride buffer, soda water / sodium bicarbonate buffer, oxalic acid / sodium hydroxide buffer, tris(hydroxymethylaminomethane) buffer, glycine buffer, 2-(4-hydroxyethyl)-1-piperazineethanesulfonic acid buffer, di(hydroxymethyl)-diamine buffer, and 3-(N-methylamino)propanesulfonic acid buffer.
[0011] Preferably, the polyphenol compound is one or a combination of two or more of catechin polyphenol compounds, anthocyanin polyphenol compounds, flavanol polyphenol compounds, flavonoid polyphenol compounds, and caffeic acid polyphenol compounds; The catechin polyphenol compound is one or a combination of two or more of (-)-catechin, (-)-epicatechin, theaflavin, thearubigin, protocatechin, (-)-epigallocatechin gallate, etc.; The anthocyanidin polyphenol compound is one or a combination of two or more of anthocyanidin, zeaxanthin, and apple xanthin; The flavanol polyphenol compound is one or a combination of two or more of quercetin, kaempferol, myricetin, isoquercetin, etc.; The flavonoid polyphenol compound is one or a combination of two or more of flavonoids, flavonols, isoflavones, coumarins, tannic acid, etc.; The caffeic acid polyphenol compound is one or a combination of two or more of caffeic acid, silymarinic acid, erythric acid, rutin, theotannic acid and the like.
[0012] Preferably, the molecular weight of the hyaluronic acid is a low molecular weight hyaluronic acid of 5 to 500 KDa.
[0013] Preferably, the protein is one or a combination of two or more of albumin, fibrinogen, type I collagen, type II collagen, type III collagen, type IV collagen, bone collagen, lysozyme, antimicrobial peptides, neuropeptides, growth factors, and whole plasma proteins; The metal compound is a compound containing any of the following metal ions: Fe 2+ , Fe 3+ 、Zn 2+ , Cu + , Cu 2+ 、Ni2+ , Ca 2+ 、Co 2+ 、Co 3+ , Mn 2+ , Mn 3+ , Mn 4+ .
[0014] Preferably, in step (1), the volume concentration of the aqueous silane coupling agent in the aqueous silane coupling agent solution is 0.1-5%; And / or, in step (2), the pH value of the alkaline buffer solution is 7.5-10; And / or, in step (2), the mass concentration of the polyphenol compound in the polyphenol solution is 0.5-10 mg / mL; the mass concentration of the thiolated hyaluronic acid in the hyaluronic acid solution is 0.1-5 mg / mL; And / or, in step (5), the mass concentration of protein in the protein solution is 0.1-100 mg / mL; the mass concentration of metal ions in the metal ion solution is 0.1-10 mg / mL.
[0015] Preferably, in step (1), the reaction time is 0.5-24 h, and the reaction temperature is 15-40° C.; And / or, in step (3), the reaction time is 1-48 hours, and the reaction temperature is 15-40°C; And / or, in step (4), the reaction time is 0.5-24 h, and the reaction temperature is 15-40° C.; And / or, in step (6), the reaction time is 1-48 hours, and the reaction temperature is 15-37°C.
[0016] Based on the same technical concept, another embodiment of the present invention is to provide a multifunctional metal-active protein coating obtained by the above preparation method.
[0017] The beneficial effects of the present invention are: 1. In order not to affect protein folding or function, a hydrophilic polymer surface must be constructed in advance, such as polyethylene glycol (PEG) and zwitterions. However, such antifouling hydrophilic surfaces have problems such as insufficient stability of the hydrophilic coating, resistance to protein adhesion, easy detachment of the adhered protein, or the need for a cumbersome preparation process, which greatly affects the preparation of the protein surface. The preparation method of the present invention is to construct a polyphenol-hyaluronic acid composite surface by a simple immersion method. A large number of hydrophilic functional groups / compounds on the surface can maintain the wettability of the coating for a long time.
[0018] 2. In the preparation process of traditional protein coatings, due to its cumbersome chemical coupling process, the protein may undergo denaturation or inactivation, thereby affecting the biological function of the coating. The preparation method of the present invention is to simply immerse the material in a physiological buffer of the protein, so that the protein can be modified on a composite surface of polyphenols and hyaluronic acid with excellent hydrophilicity, and the active groups in the coating, such as amino, carboxyl, phenolic hydroxyl, quinone, benzene ring, etc., adsorb the protein; at the same time, the rapidly formed hydration layer effectively maintains the natural conformation of the adsorbed protein, retaining the activity of the protein and the corresponding biological function.
[0019] 3. Different from the traditional surface that can only adsorb one or several specific proteins, the coating prepared by the present invention can non-specifically adsorb proteins and selectively adsorb one or several proteins according to the needs of the service environment. For example, for an anti-adhesion environment, it can adsorb a single albumin; for an antibacterial environment, it can adsorb one or several combined antibacterial proteins; for a surface that needs to regulate the growth of certain cells, it can adsorb the corresponding proteins that promote their adhesion, migration and proliferation, etc., and has a broad spectrum of protein adsorption.
[0020] 4. In the pathological tissue environment in the body, there are often a large number of active oxygen free radicals and inflammatory cell infiltration. Different from the traditional pure protein coating surface, the polyphenol-hyaluronic acid complex in the coating prepared by the present invention can not only maintain the wettability of the surface, but also play its corresponding biological functions; such as the antioxidant, anti-inflammatory and free radical scavenging effects of polyphenols, and the maintenance and repair of tissues, regulation of cell migration and proliferation, and antioxidant effects of hyaluronic acid. Under the synergistic effect of polyphenols and hyaluronic acid, the protein surface can better play the corresponding biological functions and greatly improve the therapeutic effect of medical devices.
[0021] 5. The metal ions in the present invention are chelated with phenolic hydroxyl groups and proteins at the same time, which has many functions: the biological functions of the metal ions themselves, such as antibacterial, anticoagulant, enzyme catalytic activity, immunomodulatory, anti-inflammatory and promotion of tissue repair; the chelated metal ions act as a rivet to further connect and fix the polyphenol nanoparticles, hyaluronic acid and adsorbed proteins in the coating, thereby increasing the structural stability of the entire coating; and the metal ions as cations in the coating can bind to water molecules, synergistically enhancing the anti-fouling performance of the metal-protein coating.
[0022] 6. The preparation method of the present invention is simple to operate, has efficient reaction, mild conditions, and has broad-spectrum practicability. Different proteins and metal ions can be modified on the surface of substrates of different properties and shapes, thereby preparing stable multifunctional metal-active protein coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 This is a data graph of the rate of NO release by catalytic nitric oxide donors on the surface of the Cu-VEGF active coating prepared in Example 1.
[0025] Figure 2 It is the fluorescence image of vascular endothelial cells on the Cu-VEGF active coating and the surface of the substrate material prepared in Example 1.
[0026] Figure 3 This is a data graph of the absorbance value of vascular endothelial cells adhered to the surface of the sample prepared in Example 1 detected by using a CCK-8 kit.
[0027] Figure 4 This is a graph showing the antibacterial performance of the Zn-antimicrobial peptide coating prepared on the surface of medical polyurethane in Example 2.
[0028] Figure 5 It is the fluorescence image of platelet adhesion and activation on the surfaces of different samples in Example 3 (scale bar 50 μm).
[0029] Figure 6 This is a data graph of the antibacterial rate of different sample surfaces in Example 3 detected by using a microbial kit. DETAILED DESCRIPTION
[0030] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0031] Example 1 This embodiment provides a method for preparing a multifunctional metal-active protein coating, the preparation method comprising: (1) preparing an aminoethyltriethoxysilane solution with a volume concentration of 1% with distilled water, and fully immersing 316L stainless steel in the medical metal-based material in the aminoethyltriethoxysilane solution, reacting at 20° C. for 10 hours, and then fully washing with distilled water to obtain a first reaction sample; (2) dissolving tannic acid and thiolated hyaluronic acid in a sodium bicarbonate / sodium carbonate buffer solution at pH 8, respectively, so that the mass concentrations of the tannic acid solution and the hyaluronic acid solution are 2 mg / mL and 1 mg / mL, respectively; (3) The first reaction sample obtained in step (1) is completely immersed in a tannic acid solution, reacted at 20° C. for 18 h, and then fully washed with distilled water to obtain a second reaction sample; (4) The second reaction sample obtained in step (3) is completely immersed in the thiolated hyaluronic acid solution, reacted at 20° C. for 20 h, and then fully washed with distilled water to obtain a third reaction sample.
[0032] (5) Dissolving vascular endothelial growth factor VEGF and CuCl2 with PBS solution so that the mass concentrations of sterile VEGF solution and CuCl2 solution are 0.2 mg / mL and 0.5 mg / mL, respectively; (6) Mix equal volumes of VEGF solution and CuCl2 solution to obtain a mixed solution; and completely immerse the third reaction sample in the mixed solution, react at 20°C for 24 hours, then wash and dry with nitrogen to obtain a multifunctional metal-active protein coating.
[0033] Example 2 This embodiment provides a method for preparing a multifunctional metal-active protein coating, the preparation method comprising: (1) A methyltrimethoxysilane solution with a volume concentration of 2% is prepared with distilled water, and the polyurethane material in the medical plastic-based material is fully immersed in the methyltrimethoxysilane solution, reacted at 25°C for 8 hours, and then fully washed with distilled water to obtain a first reaction sample.
[0034] (2) Dissolving (-)-epigallocatechin gallate and thiolated hyaluronic acid in trimethylamine / hydrochloric acid buffer at pH 8, respectively, such that the mass concentrations of (-)-epigallocatechin gallate solution and thiolated hyaluronic acid solution are 3 mg / mL and 1.5 mg / mL, respectively; (3) The first reaction sample obtained in step (1) is completely immersed in a (-)-epigallocatechin gallate solution, reacted at 25° C. for 12 h, and then fully washed with distilled water to obtain a second reaction sample; (4) The second reaction sample obtained in step (3) is completely immersed in the thiolated hyaluronic acid solution, reacted at 25° C. for 18 h, and washed thoroughly with distilled water to obtain a third reaction sample.
[0035] (5) Dissolving the antimicrobial peptide and ZnCl2 in PBS solution to make the mass concentrations of the antimicrobial peptide solution and ZnCl2 solution 5 mg / mL and 0.5 mg / mL, respectively; (6) Mix equal volumes of the antimicrobial peptide solution and the ZnCl2 solution to obtain a mixed solution; and completely immerse the third reaction sample in the mixed solution, react at 25°C for 8 h, and then rinse thoroughly with distilled water and dry with nitrogen to obtain a multifunctional metal-active protein coating.
[0036] Example 3 This embodiment provides a method for preparing a multifunctional metal-active protein coating, the preparation method comprising: (1) preparing a 3% volume concentration of trimethoxysilane acrylate solution with distilled water, and fully immersing the polylactic acid material in the medical plastic-based material in the trimethoxysilane acrylate solution, reacting at 30° C. for 12 hours, and then fully washing with distilled water to obtain a first reaction sample; (2) dissolving anthocyanin and thiolated hyaluronic acid in a phosphate buffer solution at pH 8, respectively, so that the mass concentrations of the anthocyanin solution and the thiolated hyaluronic acid solution are 5 mg / mL and 3 mg / mL, respectively; (3) The first reaction sample obtained in step (1) is completely immersed in the anthocyanin solution, reacted at 30° C. for 8 h, and then fully washed with distilled water to obtain a second reaction sample; (4) The second reaction sample obtained in step (3) is completely immersed in the thiolated hyaluronic acid solution, reacted at 30° C. for 12 h, and then fully washed with distilled water to obtain a third reaction sample.
[0037] (5) Dissolve bovine serum albumin and AgNO3 in PBS solution to make the mass concentrations of bovine serum albumin solution and AgNO3 solution be 10 mg / mL and 2 mg / mL respectively; (6) Mix equal volumes of bovine serum albumin solution and AgNO3 solution to obtain a mixed solution; and completely immerse the third reaction sample in the mixed solution, react at 30°C for 5 hours, and then rinse thoroughly with distilled water and dry with nitrogen to obtain a multifunctional metal-active protein coating.
[0038] Example 4 This embodiment provides a method for preparing a multifunctional metal-active protein coating, the preparation method comprising: (1) preparing an ethoxytrimethoxysilane solution with a volume concentration of 1.5% with distilled water, and fully immersing the zirconium oxide material of the medical ceramic-based material in the ethoxytrimethoxysilane solution, reacting at 35° C. for 5 hours, and then fully washing with distilled water to obtain a first reaction sample; (2) Dissolving quercetin and thiolated hyaluronic acid in glycine buffer at pH 9.5, respectively, to make the mass concentrations of quercetin solution and thiolated hyaluronic acid solution 1 mg / mL and 2 mg / mL, respectively; (3) The zirconium oxide material obtained in step (1) is completely immersed in the quercetin solution, reacted at 35° C. for 5 h, and then fully washed with distilled water to obtain a second reaction sample; (4) The sample obtained in step (3) is completely immersed in the thiolated hyaluronic acid solution, reacted at 35° C. for 4 hours, and then fully washed with distilled water to obtain a second reaction sample; (5) Dissolve collagen and CaCl2 in PBS solution to make the mass concentrations of collagen solution and CaCl2 solution 3 mg / mL and 0.4 mg / mL, respectively; (6) Mix equal volumes of lysozyme solution and CaCl2 solution, and completely immerse the third reaction sample in the mixed solution. After reacting at 35°C for 4 h, rinse thoroughly with distilled water and dry with nitrogen to obtain a multifunctional metal-active protein coating.
[0039] Experimental example like Figure 1 As shown, copper has the ability to catalyze the release of nitric oxide from nitric oxide donors, so the rate of nitric oxide release from the Cu-VEGF active coating prepared in Example 1 catalyzed by sulfur-nitrosothiol, a nitric oxide donor, was monitored in real time using a nitric oxide detector NOA 280i. Figure 1 It was found that the Cu-VEGF active coating can effectively catalyze the release of nitric oxide from the donor, with a release rate of (5.0±0.25)×10 −10 mol cm −2 min −1 , within the physiological concentration range of nitric oxide released by healthy vascular endothelial cells, indicating that the metal copper ions were successfully modified onto the coating surface and endowed the surface with the function of releasing nitric oxide by bionic vascular endothelial cells.
[0040] like Figure 2 As shown in the figure, VEGF can bind to receptors on vascular endothelial cells and regulate the proliferation, migration and lumen formation of endothelial cells through various signaling pathways, such as Ras-MAPK, PI3K-Akt and Rho GTPase, thereby playing an important role in angiogenesis and maintaining the normal function of blood vessels. Therefore, vascular endothelial cells were cultured with unmodified and Cu-VEGF active coating modified 316L stainless steel for 3 days, and the growth behavior of endothelial cells on the surfaces of the two samples was qualitatively evaluated by fluorescence staining. From the laser confocal image results, it can be found that compared with the unmodified stainless steel surface, the stainless steel surface modified with Cu-VEGF active coating can significantly promote the adhesion and growth of endothelial cells.
[0041] Subsequently, the CCK-8 kit was used to further detect the growth status of surface-adherent endothelial cells, where the CCK-8 absorbance value was positively correlated with the number and activity of adherent endothelial cells; Figure 3 As shown, the absorbance value of endothelial cells adhered to the surface of the Cu-VEGF active coating reached 2.6, while the absorbance value of the unmodified surface was only about 1.2, indicating that the active protein VEGF was successfully modified to the surface of the material, and the prepared Cu-VEGF active coating can effectively promote the proliferation of vascular endothelial cells on the surface of the material and improve their activity.
[0042] like Figure 4 As shown, the antibacterial performance of the Zn-antimicrobial peptide active coating prepared in Example 2 was tested by contact sterilization experiment. 7 The bacteria with CFU / mL were cultured with polyurethane and Zn-antimicrobial peptide coating for 6 hours, and then the adhered live bacteria were plated and cultured for another 24 hours. From the experimental results, it can be found that there are a large number of live bacteria on the polyurethane surface, while there are basically no live bacteria on the Zn-antimicrobial peptide coating surface, indicating that the prepared Zn-antimicrobial peptide active coating can significantly improve the antibacterial properties of the material.
[0043] like Figure 5 As shown, the blood compatibility of the Ag-albumin active coating prepared in Example 3 was tested by platelet adhesion experiment. Platelet-rich plasma was incubated with the base material polylactic acid and the polylactic acid modified by the Ag-albumin active coating for 4 hours, and then the adhesion of the surface platelets was observed by laser confocal microscopy and photographed; from the fluorescence image of the platelets, it was found that a large number of platelets adhered to the surface of the polylactic acid, and the adhered platelets were in an activated spreading state, while only a very small number of platelets adhered to the surface of the Ag-albumin active coating, indicating that the prepared coating surface can effectively inhibit the adhesion and activation of platelets, giving the material surface excellent blood compatibility.
[0044] like Figure 6 As shown, the concentration is 2.0×10 7 Bacteria with CFU / mL were cultured with polylactic acid and polylactic acid modified with Ag-albumin coating for 6 hours, respectively, and then the antibacterial rate of the surface was detected with a microbial kit. From the antibacterial rate results, it was found that the antibacterial rate of unmodified polylactic acid was only 25%, while the modification of Ag-albumin coating increased the antibacterial rate of the surface to 99.9%, proving that the prepared Ag-albumin coating can significantly improve the antibacterial ability of the material surface.
[0045] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a multifunctional metal-active protein coating, characterized in that: The preparation method is: (1) mixing and dissolving an aqueous silane coupling agent with water to obtain an aqueous silane coupling agent solution; and immersing a substrate material in the aqueous silane coupling agent solution to react to obtain a first reaction sample; (2) dissolving the polyphenol compound and the thiolated hyaluronic acid in an alkaline buffer solution to obtain a polyphenol solution and a hyaluronic acid solution, respectively; (3) immersing the first reaction sample obtained in step (1) in the polyphenol solution for reaction to obtain a second reaction sample; (4) immersing the second reaction sample in the hyaluronic acid solution to react, thereby obtaining a third reaction sample; (5) Dissolving the protein and the metal compound in PBS solution to obtain a protein solution and a metal ion solution, respectively; (6) mixing equal volumes of the protein solution and the metal ion solution to obtain a mixed solution; The third reaction sample is completely immersed in the mixed solution to react, thereby obtaining a multifunctional metal-active protein coating.
2. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (1), the water-based silane coupling agent is one or a combination of two or more of an aminosilane coupling agent, a methylsilane coupling agent, an acrylic silane coupling agent, and an ethoxysilane coupling agent; The aminosilane coupling agent is one or a combination of two or more of aminomethyltriethoxysilane, aminoethyltriethoxysilane, aminoethyltrimethoxysilane and aminopropyltrimethoxysilane; The methylsilane coupling agent is one or a combination of two or more of methyltrimethoxysilane, methyltriethoxysilane and methyltriisopropoxysilane; The acrylic silane coupling agent is one or a combination of two or more of acrylic trimethoxysilane, acrylic triethoxysilane, and acrylic triisopropoxysilane; The ethoxysilane coupling agent is one or a combination of two or more of ethoxytrimethoxysilane, ethoxytriethoxysilane and ethoxymethyltrimethoxysilane.
3. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (1), the base material is one of a medical metal-based material, a medical ceramic-based material, a medical polymer-based material or a medical composite material.
4. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (2), the alkaline buffer is one of sodium bicarbonate / sodium carbonate buffer, trimethylamine / hydrochloric acid buffer, phosphate buffer, ammonia / ammonium chloride buffer, soda water / sodium bicarbonate buffer, oxalic acid / sodium hydroxide buffer, tris(hydroxymethyl)aminomethane buffer, glycine buffer, 2-(4-hydroxyethyl)-1-piperazineethanesulfonic acid buffer, di(hydroxymethyl)-diamine buffer, and 3-(N-methylamino)propanesulfonic acid buffer.
5. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (2), the polyphenol compound is one or a combination of two or more of catechin polyphenol compounds, anthocyanin polyphenol compounds, flavanol polyphenol compounds, flavonoid polyphenol compounds, and caffeic acid polyphenol compounds; The catechin polyphenol compound is one or a combination of two or more of (-)-catechin, (-)-epicatechin, theaflavins, thearubigins, protocatechins, and (-)-epigallocatechin gallate; The anthocyanidin polyphenol compound is one or a combination of two or more of anthocyanidin, zeaxanthin, and apple xanthin; The flavanol polyphenol compound is one or a combination of two or more of quercetin, kaempferol, myricetin and isoquercetin; The flavonoid polyphenol compound is one or a combination of two or more of flavonoids, flavonols, isoflavones, coumarins, and tannic acid; The caffeic acid polyphenol compound is one or a combination of two or more of caffeic acid, silymarin, erythrin, rutin and theotannic acid.
6. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (2), the molecular weight of the hyaluronic acid is a low molecular weight hyaluronic acid of 5 to 500 KDa.
7. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (5), the protein is one or a combination of two or more of albumin, fibrinogen, type I collagen, type II collagen, type III collagen, type IV collagen, bone collagen, lysozyme, antimicrobial peptides, neuropeptides, growth factors, and whole plasma proteins; And / or, the metal compound is a compound containing any of the following metal ions: Fe 2+ , Fe 3+ 、Zn 2+ , Cu + , Cu 2 + 、Ni 2+ , Ca 2+ 、Co 2+ 、Co 3+ , Mn 2+ , Mn 3+ , Mn 4+ .
8. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (1), the volume concentration of the aqueous silane coupling agent in the aqueous silane coupling agent solution is 0.1-5%; And / or, in step (2), the pH value of the alkaline buffer solution is 7.5-10; And / or, in step (2), the mass concentration of the polyphenol compound in the polyphenol solution is 0.5-10 mg / mL; the mass concentration of the thiolated hyaluronic acid in the hyaluronic acid solution is 0.1-5 mg / mL; And / or, in step (5), the mass concentration of protein in the protein solution is 0.1-100 mg / mL; the mass concentration of metal ions in the metal ion solution is 0.1-10 mg / mL.
9. The method for preparing the multifunctional metal-active protein coating according to claim 1, characterized in that: In step (1), the reaction time is 0.5-24 h, and the reaction temperature is 15-40° C.; And / or, in step (3), the reaction time is 1-48 hours, and the reaction temperature is 15-40°C; And / or, in step (4), the reaction time is 0.5-24 h, and the reaction temperature is 15-40° C.; And / or, in step (6), the reaction time is 1-48 hours, and the reaction temperature is 15-37°C.
10. The multifunctional metal-active protein coating obtained by the preparation method according to any one of claims 1 to 9.