Bipolar membrane capable of stably transmitting ions and preparation method of bipolar membrane
The gradient intermediate layer is prepared through dual-channel electrospinning technology, which solves the problems of complexity and high cost of improving the intermediate interface layer in the existing technology, realizes a simple-to-operate, low-cost bipolar membrane with stable ion transmission, and improves the performance of bipolar membranes. Interfacial bonding strength and ion transport efficiency.
Patent Information
- Application Number
- CN202411168337.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-22
AI Technical Summary
The existing methods of improving the intermediate interface layer of bipolar membranes mainly rely on the synthesis of new catalysts, which are complex operations, high costs and limited application scope.
The gradient intermediate layer is prepared through dual-channel electrospinning technology, and the ratio of cation exchange resin and anion exchange resin in the fiber is dynamically adjusted to form a gradient ratio composite fiber to improve the ion exchange capacity of the intermediate layer, and a catalyst is sprayed during the spinning process to Evenly dispersed, enhancing the interfacial compatibility and ion transmission efficiency of the bipolar membrane.
A bipolar membrane with stable ion transmission that is simple to operate, low in cost and widely used has been realized, which improves the interface bonding strength and ion transmission efficiency of the bipolar membrane and ensures mechanical strength and flexibility.
Smart Images

Figure CN118807487A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bipolar membrane preparation, in particular to a bipolar membrane for stable ion transmission and a preparation method thereof. Background Art
[0002] Bipolar membrane is a new type of ion exchange composite membrane, which usually includes an anion selective layer, a cation selective layer and an intermediate interface layer between the two membrane layers. Under the action of a reverse bias electric field, the bipolar membrane can efficiently dissociate water into hydrogen ions and hydroxide ions, thereby converting the salt in the aqueous solution into the corresponding acid and base. Electrodialysis based on bipolar membrane has the advantages of simplicity, high efficiency, energy saving and cleanliness, and has broad applications in pollution control, resource recovery and chemical production processes, especially the production of organic acids.
[0003] The middle interface layer of the bipolar membrane is the area where water dissociates in the bipolar membrane, which has a crucial impact on the performance of the bipolar membrane. A bipolar membrane with excellent performance can be prepared by improving the middle interface layer. At present, the improvement of the middle interface layer is mainly achieved by changing the type of catalyst and the preparation process, such as Chinese patents CN1704151A and CN1727058A. These methods of improving the performance of the middle interface layer by synthesizing new catalysts are not only complicated to operate, costly, but also limited in scope of application.
[0004] Therefore, the present invention proposes a breakthrough and universal improvement to the intermediate layer, which gives the intermediate layer a gradual ion exchange capacity and provides smoother ion transfer and better mechanical integration between the anion exchange membrane and the cation exchange membrane. The present invention does not require the synthesis of new materials, is simple to operate, has extremely low cost, and is widely used. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a bipolar membrane with stable ion transport, which is used to solve the problem that the prior art generally improves the interface intermediate layer by synthesizing new catalysts, which is not only complicated to operate, but also costly and has a limited scope of application. At the same time, the present invention will also provide a method for preparing a bipolar membrane with stable ion transport.
[0006] In order to achieve the above-mentioned object and other related objects, the present invention provides the following technical solutions: According to a first aspect of the present invention, a bipolar membrane for stable ion transport is provided, the bipolar membrane comprising a cation exchange membrane, an anion exchange membrane and a gradient intermediate layer; the gradient intermediate layer is a multilayer fiber structure prepared by dual-channel electrospinning of spinning solution A and spinning solution B, and when preparing each layer of fiber, the ratio of spinning solution A to spinning solution B gradually changes from 1:0 to 0:1 or from 0:1 to 1:0, the spinning solution A contains a cation exchange resin, and the spinning solution B contains an anion exchange resin; the cation exchange membrane is arranged on the side of the gradient intermediate layer containing a high proportion of cation exchange resin, and the anion exchange membrane is arranged on the other side of the gradient intermediate layer.
[0007] The present invention adjusts the ratio of cation exchange resin to anion exchange resin in each layer of fiber by dynamically adjusting the output ratio of the dual channels, thereby preparing anion-cation composite fibers with a gradient ratio, so that the gradient middle layer has a gradient ion exchange capacity, which can not only improve the interface compatibility between the gradient middle layer and the cation exchange membrane and the anion exchange membrane, and enhance the interface bonding strength of the bipolar membrane; it can also promote smoother and more stable transfer between ions, and enhance the ion transmission efficiency.
[0008] Furthermore, the thickness of the gradient intermediate layer is between 5 and 50 microns. This thickness range can ensure that the gradient intermediate layer has sufficient mechanical strength without sacrificing too much ion transfer efficiency.
[0009] During the electrospinning process, the thickness of each fiber layer is between 1 and 10 microns, and the number of layers is between 5 and 12. This thickness range allows enough exchange resin to exist in each layer to achieve ion exchange function, while being thin enough to maintain the flexibility and lightness of the bipolar membrane as a whole.
[0010] Furthermore, the ratio of spinning solution A to spinning solution B in each layer of fiber gradually changes from 1:0 to 0.5:0.5 and then to 0:1, or gradually changes from 0:1 to 0.5:0.5 and then to 1:0.
[0011] Furthermore, the gradient middle layer is a 5-layer fiber structure. When preparing each layer of fiber, the ratios of spinning solution A and spinning solution B are 1:0, 0.75:0.25, 0.5:0.5, 0.25:0.75, and 0:1, or 0:1, 0.25:0.75, 0.5:0.5, 0.75:0.25, and 1:0.
[0012] Furthermore, the gradient middle layer has a 6-layer fiber structure. When preparing each layer of fiber, the ratios of spinning solution A and spinning solution B are 1:0, 0.8:0.2, 0.6:0.4, 0.4:0.6, 0.2:0.8, and 0:1, or 0:1, 0.2:0.8, 0.4:0.6, 0.6:0.4, 0.8:0.2, and 1:0, respectively.
[0013] Furthermore, the gradient middle layer is a fiber structure of 11 layers. When preparing each layer of fiber, the ratio of spinning solution A to spinning solution B is 1:0, 0.9:0.1, 0.8:0.2, 0.7:0.3, 0.6:0.4, 0.5:0.5, 0.4:0.6, 0.3:0.7, 0.2:0.8, 0.1:0.9, 0:1, or 0:1, 0.1:0.9, 0.2:0.8, 0.3:0.7, 0.4:0.6, 0.5:0.5, 0.6:0.4, 0.7:0.3, 0.8:0.2, 0.9:0.1, 1:0.
[0014] Further, the cation exchange groups contained in the cation exchange resin include at least one of sulfonic acid group, carboxyl group, phosphonic acid group, phosphinic acid group, arsenic acid group and selenic acid group; The anion exchange groups contained in the anion exchange resin include at least one of quaternary ammonium salts, primary amines, secondary amines, tertiary amines, and tertiary sulfonium groups.
[0015] Furthermore, the concentration of the cation exchange resin in the spinning solution A is 1-25% (w / v), and the concentration of the anion exchange resin in the spinning solution B is 1-25% (w / v).
[0016] Furthermore, the concentration of the cation exchange resin in the spinning solution A is consistent with the concentration of the anion exchange resin in the spinning solution B.
[0017] Furthermore, the spinning solution A / spinning solution B also contains a binder and a diluent.
[0018] Furthermore, the adhesive includes at least one of polyacrylonitrile, polyethylene, polyvinyl chloride, polyvinyl alcohol, fluororubber, styrene-butadiene rubber, cellulose derivatives, polytetrafluoroethylene, polychlorotrifluoroethylene, polyvinylidene fluoride, polysulfone, polyetheretherketone, styrene-ethylene-butylene-styrene and polyphenylene ether.
[0019] Furthermore, the concentration of the binder is 1-10% (w / v).
[0020] Furthermore, the diluent includes at least one of water, methanol, ethanol, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide.
[0021] Furthermore, the spinning solution A / spinning solution B also contains a spinning aid, and the spinning aid includes at least one of polyethylene oxide, polyacrylic acid, polyvinyl pyrrolidone, and polyvinyl alcohol.
[0022] Furthermore, the spinning solution A / spinning solution B also contains a nonionic surfactant. By adding a nonionic surfactant, the surface area effect of the spinning solution can be reduced, the spinning effect can be improved, and the diameter of the fiber can be greatly reduced.
[0023] Furthermore, the nonionic surfactant includes at least one of isomeric alcohol polyoxyethylene polyoxypropylene ether, alkylphenol polyoxyethylene ether, and alkyl alcohol amide.
[0024] Furthermore, the concentration of the nonionic surfactant is 0.05-0.30% (w / v).
[0025] Furthermore, the interior and surface of the gradient middle layer are loaded with a catalyst; the catalyst is sprayed onto the gradient middle layer during the spinning process.
[0026] Furthermore, the catalyst includes at least one of aluminum hydroxide, graphene oxide, and titanium dioxide.
[0027] A second aspect of the present invention provides a method for preparing a bipolar membrane for stable ion transport, comprising the following steps: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared and injected into micro-injection pump 1 and micro-injection pump 2 of a dual-channel electrospinning device respectively to prepare a multi-layer fiber structure. Micro-injection pump 1 and micro-injection pump 2 are controlled separately. The flow rates of micro-injection pump 1 and micro-injection pump 2 are dynamically adjusted to gradually change the ratio of cation exchange resin to anion exchange resin in each layer of fiber from 1:0 to 0:1 (or from 0:1 to 1:0). Meanwhile, during the spinning process of the gradient middle layer, a dispersion of a catalyst is continuously or periodically electrosprayed to obtain a gradient middle layer. (2) Preparation of bipolar membrane: The gradient middle layer is stacked together with the cation exchange membrane and the anion exchange membrane, wherein the cation exchange membrane is located on the side of the gradient middle layer with a high proportion of cation exchange resin, and the anion exchange membrane is located on the other side of the gradient middle layer, and then passed back and forth in a hot roller machine several times to obtain the bipolar membrane.
[0028] Furthermore, in step (1), the catalyst dispersion is continuously or periodically electrosprayed during the preparation of the gradient intermediate layer. By spraying the catalyst during the spinning process, the catalyst can be uniformly attached to the fiber, thereby being uniformly dispersed inside and on the surface of the gradient intermediate layer, effectively preventing the formation of agglomerated large particles and improving the ion transmission efficiency and stability of the bipolar membrane.
[0029] Furthermore, in step (1), during electrospinning, the electrospinning voltage is 8 to 30 kV and the nozzle distance is 10 to 15 cm.
[0030] Furthermore, in step (1), the flow rate of the microinjection pump 1 is controlled between 0.0-1.0 mL / h (or between 1.0-0.0 mL / h), and the flow rate of the microinjection pump 2 is synchronously controlled between 1.0-0 mL / h (or between 0-1.0 mL / h).
[0031] Furthermore, in step (2), spraying a water / alcohol solution on the prepared gradient intermediate layer can soften the fiber layer to obtain a better hot pressing effect. Compared with solvent vapor treatment, it can reduce the processing time, improve production efficiency and reduce production costs.
[0032] Furthermore, in step (2), the anion exchange membrane and the cation exchange membrane are prepared separately by a solution-based membrane laying method or commercial anion exchange membrane and commercial cation exchange membrane are used.
[0033] Furthermore, in step (2), anion exchange resins and cation exchange resins are respectively prepared into anion membrane casting solution and cation membrane casting solution, and the anion membrane casting solution and the cation membrane casting solution are respectively evenly coated on a pre-cleaned and treated substrate using a solution film laying method, and after complete drying, anion exchange membrane and cation exchange membrane are obtained.
[0034] As described above, the bipolar membrane for stable ion transport and the preparation method thereof of the present invention have the following beneficial effects: 1. The present invention prepares anion-cation composite fibers with a gradient ratio by gradually changing the ratio of anion-cation exchange resins in each layer of fiber of the gradient intermediate layer, so that the gradient intermediate layer has a gradient ion exchange capacity, which can not only improve the interface compatibility between the gradient intermediate layer and the cation exchange membrane and the anion exchange membrane, and enhance the interface bonding strength of the bipolar membrane; it can also promote smoother and more stable transfer between ions, and enhance the ion transmission efficiency.
[0035] 2. The present invention creatively proposes to improve the preparation method of the intermediate layer, giving the intermediate layer a gradient ion exchange capacity, providing smoother ion transfer and better mechanical integration between the anion exchange membrane and the cation exchange membrane; the present invention is simple to operate, extremely low in cost, and widely used.
[0036] 3. In the process of preparing the gradient intermediate layer, the present invention continuously or periodically electrosprays the catalyst dispersion liquid, so that the catalyst particles are evenly dispersed inside and on the surface of the gradient intermediate layer, preventing the formation of agglomerated large particles and improving the ion transmission efficiency and stability of the bipolar membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 Shown is an electron microscope image of the graded interlayer disclosed in Example 1 of the present invention.
[0038] Figure 2 Shown is an electron microscope image of the intermediate layer disclosed in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0040] Example 1 A bipolar membrane for stable ion transmission, the preparation method of which comprises the following steps: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared, wherein spinning solution A comprises 5% w / v sodium polystyrene sulfonate (PSS), 2% w / v polyvinyl alcohol (PVA), and the balance is water; spinning solution B comprises 5% w / v polyallylamine chloride (PAC), 2% w / v polyvinyl alcohol (PVA), and the balance is water; The spinning solution A and the spinning solution B are respectively injected into the microinjection pump 1 and the microinjection pump 2 of the dual-channel electrospinning equipment to prepare a multilayer fiber structure. At the same time, the dispersion of aluminum hydroxide is continuously electrosprayed during the spinning process. The microinjection pump 1 and the microinjection pump 2 are controlled separately. The flow rate of the microinjection pump 1 is adjusted to 0, 0.2, 0.4, 0.6, 0.8, and 1.0 mL / h, and the flow rate of the microinjection pump 2 is synchronously adjusted to 1.0, 0.8, 0.6, 0.4, 0.2, and 0 mL / h, respectively. The thickness of each layer is 5 microns, and there are 6 layers in total. After drying, a gradient middle layer is obtained.
[0041] The gradient intermediate layer is photographed using a scanning electron microscope. Figure 1 As shown, the gradient middle layer is evenly distributed and no particle agglomeration is observed.
[0042] (2) Preparation of bipolar membrane: The gradient middle layer was stacked together with a commercial cation exchange membrane (135 μm thick) and a commercial anion exchange membrane (135 μm thick), wherein the cation exchange membrane was located on the side of the gradient middle layer having a high PSS ratio and the anion exchange membrane was located on the other side, and then passed back and forth in a hot roller machine three times to obtain the bipolar membrane.
[0043] After testing, when the current density is 100 mA / cm 2 When the voltage drop across the bipolar membrane is only 1.0V.
[0044] Example 2 A bipolar membrane for stable ion transmission, the preparation method of which comprises the following steps: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared, wherein spinning solution A comprises 5% w / v sodium polystyrene sulfonate (PSS), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v isomeric alcohol polyoxyethylene polyoxypropylene ether, and the balance is water; spinning solution B comprises 5% w / v polyallylamine chloride (PAC), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v isomeric alcohol polyoxyethylene polyoxypropylene ether, and the balance is water; Spinning solution A and spinning solution B are respectively injected into micro-injection pump 1 and micro-injection pump 2 of the dual-channel electrospinning device to prepare a multi-layer fiber structure, and aluminum hydroxide dispersion is continuously electrosprayed during the spinning process. Micro-injection pump 1 and micro-injection pump 2 are controlled separately, and the flow rate of micro-injection pump 1 is adjusted to 0, 0.2, 0.4, 0.6, 0.8, 1.0 mL / h, and the flow rate of micro-injection pump 2 is synchronously adjusted to 1.0, 0.8, 0.6, 0.4, 0.2, 0 mL / h, each layer is 5 microns thick, and a total of 6 layers are obtained. After drying, a gradient middle layer is obtained; (2) Preparation of bipolar membrane: The gradient middle layer was stacked with a commercial cation exchange membrane (135 microns thick) and a commercial anion exchange membrane (135 microns thick), the cation exchange membrane was located on the side of the gradient middle layer with a high PSS ratio, and the anion exchange membrane was located on the other side, and then passed back and forth in a hot roller machine for 3 times to obtain the bipolar membrane. After testing, when the current density was 100 mA / cm 2 When the voltage drop across the bipolar membrane is only 0.89V.
[0045] Example 3 A bipolar membrane for stable ion transmission, the preparation method of which comprises the following steps: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared, wherein spinning solution A comprises 5% w / v sodium polystyrene sulfonate (PSS), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v isomeric alcohol polyoxyethylene polyoxypropylene ether, and the balance is water; spinning solution B comprises 5% w / v polyallylamine chloride (PAC), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v isomeric alcohol polyoxyethylene polyoxypropylene ether, and the balance is water; Spinning solution A and spinning solution B are respectively injected into micro-injection pump 1 and micro-injection pump 2 of the dual-channel electrospinning device to prepare a multi-layer fiber structure, and aluminum hydroxide dispersion is continuously electrosprayed during the spinning process. Micro-injection pump 1 and micro-injection pump 2 are controlled separately, and the flow rate of micro-injection pump 1 is adjusted to 0, 0.25, 0.5, 0.75, 1.0 mL / h, and the flow rate of micro-injection pump 2 is synchronously adjusted to 1.0, 0.75, 0.5, 0.25, 0 mL / h, each layer is 5 microns thick, and a total of 5 layers are obtained. After drying, a gradient middle layer is obtained; (2) Preparation of bipolar membrane: The gradient middle layer was stacked with a commercial cation exchange membrane and a commercial anion exchange membrane, the cation exchange membrane was located on the side of the gradient middle layer with a high PSS ratio, and the anion exchange membrane was located on the other side, and then passed back and forth in a hot roller machine for 3 times to obtain the bipolar membrane. After testing, when the current density was 100 mA / cm 2 When the bipolar membrane is energized, the transmembrane voltage drop is only 0.94V.
[0046] Example 4 A bipolar membrane for stable ion transmission, the preparation method of which comprises the following steps: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared, wherein spinning solution A comprises 5% w / v sodium polystyrene sulfonate (PSS), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v alkylphenol polyoxyethylene ether, and the balance is water; spinning solution B comprises 5% w / v polyallylamine chloride (PAC), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v alkylphenol polyoxyethylene ether, and the balance is water; Spinning solution A and spinning solution B are respectively injected into micro-injection pump 1 and micro-injection pump 2 of the dual-channel electrospinning device to prepare a multi-layer fiber structure, and aluminum hydroxide dispersion is continuously electrosprayed during the spinning process. Micro-injection pump 1 and micro-injection pump 2 are controlled separately, and the flow rate of micro-injection pump 1 is adjusted to 0, 0.25, 0.5, 0.75, 1.0 mL / h, and the flow rate of micro-injection pump 2 is synchronously adjusted to 1.0, 0.75, 0.5, 0.25, 0 mL / h, each layer is 5 microns thick, and a total of 5 layers are obtained. After drying, a gradient middle layer is obtained; (2) Preparation of bipolar membrane: The gradient middle layer was stacked with a commercial cation exchange membrane and a commercial anion exchange membrane, the cation exchange membrane was located on the side of the gradient middle layer with a high PSS ratio, and the anion exchange membrane was located on the other side, and then passed back and forth in a hot roller machine for 3 times to obtain the bipolar membrane. After testing, when the current density was 100 mA / cm 2 When the bipolar membrane is energized, the voltage drop across the membrane is only 0.99 V.
[0047] Example 5 A bipolar membrane for stable ion transmission, the preparation method of which comprises the following steps: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared, wherein spinning solution A comprises 5% w / v sodium polystyrene sulfonate (PSS), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v isomeric alcohol polyoxyethylene polyoxypropylene ether, and the balance is DMF; spinning solution B comprises 5% w / v polyallylamine chloride (PAC), 2% w / v polyvinyl alcohol (PVA), 0.1% w / v isomeric alcohol polyoxyethylene polyoxypropylene ether, and the balance is DMF; Spinning solution A and spinning solution B are respectively injected into the micro-injection pump 1 and the micro-injection pump 2 of the dual-channel electrospinning device to prepare a multi-layer fiber structure, and the dispersion of graphene oxide is continuously electrosprayed during the spinning process. The micro-injection pump 1 and the micro-injection pump 2 are controlled separately, and the flow rate of the micro-injection pump 1 is adjusted to 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 mL / h, and the flow rate of the micro-injection pump 2 is synchronously adjusted to 1.0, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1, 0 mL / h, each layer is 2 microns thick, and there are 11 layers in total. After drying, a gradient middle layer is obtained; (2) Preparation of bipolar membrane: The gradient middle layer was stacked with a commercial cation exchange membrane and a commercial anion exchange membrane, the cation exchange membrane was located on the side of the gradient middle layer with a high PSS ratio, and the anion exchange membrane was located on the other side, and then passed back and forth in a hot roller machine for 3 times to obtain the bipolar membrane. After testing, when the current density was 100 mA / cm 2 When the bipolar membrane is energized, the voltage drop across the membrane is only 0.85 V.
[0048] Comparative Example 1 A bipolar membrane, the preparation method of which comprises the following steps: (1) Preparation of the intermediate layer: Spinning solution A and spinning solution B are prepared, wherein spinning solution A comprises 5% w / v sodium polystyrene sulfonate (PSS), 2% w / v polyvinyl alcohol (PVA), and the balance is water; spinning solution B comprises 5% w / v polyallylamine chloride (PAC), 2% w / v polyvinyl alcohol (PVA), and the balance is water; Spinning solution A and spinning solution B are electrospun into a cationic fiber layer and an anionic fiber layer with a thickness of 15 microns, respectively. A dispersion of aluminum hydroxide is electrosprayed on the surface of the cationic fiber layer. The cationic fiber layer and the anionic fiber layer are then stacked and hot-pressed to obtain an intermediate layer.
[0049] The intermediate layer was imaged using a scanning electron microscope, such as Figure 2 As shown, large particles of aluminum hydroxide agglomerate in the middle of the middle layer.
[0050] (2) Preparation of bipolar membrane: The intermediate layer was stacked with a commercial cation exchange membrane on one side of the cation fiber layer and a commercial anion exchange membrane on the other side, and then passed back and forth in a hot roller machine three times to obtain the bipolar membrane.
[0051] After testing, when the current density is 100 mA / cm 2 When the voltage across the bipolar membrane drops to 2.5V.
[0052] In summary, the present invention gradually changes the ratio of anion and cation exchange resins in each layer of fiber in the gradient intermediate layer, thereby preparing anion and cation composite fibers with a gradient ratio, giving the intermediate layer a gradient ion exchange capacity, which can not only improve the interface compatibility between the gradient intermediate layer and the cation exchange membrane and the anion exchange membrane, and improve the interface bonding strength of the bipolar membrane; it can also promote smoother and more stable transfer between ions, and improve the ion transmission efficiency. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.
[0053] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A bipolar membrane for stable ion transport, characterized in that: The bipolar membrane includes a cation exchange membrane, an anion exchange membrane and a gradient intermediate layer; the gradient intermediate layer is a multi-layer fiber structure prepared by dual-channel electrospinning of spinning solution A and spinning solution B, and when preparing each layer of fiber, the ratio of spinning solution A to spinning solution B gradually changes from 1:0 to 0:1 or from 0:1 to 1:0, the spinning solution A contains a cation exchange resin, and the spinning solution B contains an anion exchange resin; the cation exchange membrane is arranged on the side of the gradient intermediate layer with a high proportion of cation exchange resin, and the anion exchange membrane is arranged on the other side of the gradient intermediate layer.
2. The bipolar membrane for stable ion transport according to claim 1, characterized in that: The thickness of the gradient middle layer is between 5 and 50 microns; the thickness of each layer of fiber in the gradient middle layer is between 1 and 10 microns, and the number of layers is between 5 and 12.
3. The bipolar membrane for stable ion transport according to claim 1, characterized in that: The ratio of spinning solution A to spinning solution B in each layer of fiber in the gradient middle layer gradually changes from 1:0 to 0.5:0.5 and then to 0:1, or gradually changes from 0:1 to 0.5:0.5 and then to 1:
0.
4. The bipolar membrane for stable ion transport according to claim 1, characterized in that: The cation exchange groups contained in the cation exchange resin include at least one of sulfonic acid group, carboxyl group, phosphonic acid group, phosphinic acid group, arsenic acid group and selenic acid group; The anion exchange groups contained in the anion exchange resin include at least one of quaternary ammonium salts, primary amines, secondary amines, tertiary amines, and tertiary sulfonium groups.
5. The bipolar membrane for stable ion transport according to claim 1, characterized in that: The spinning solution A / spinning solution B also contains a binder and a diluent.
6. The bipolar membrane for stable ion transport according to claim 5, characterized in that: The spinning solution A / spinning solution B also contains a spinning aid, and the spinning aid includes at least one of polyethylene oxide, polyacrylic acid, polyvinyl pyrrolidone, and polyvinyl alcohol.
7. The bipolar membrane for stable ion transport according to claim 5, characterized in that: The spinning solution A / spinning solution B also contains a nonionic surfactant, and the nonionic surfactant includes at least one of isomeric alcohol polyoxyethylene polyoxypropylene ether, alkylphenol polyoxyethylene ether, and alkyl alcohol amide.
8. The bipolar membrane for stable ion transport according to claim 1, characterized in that: The interior and surface of the gradient intermediate layer are loaded with a catalyst; the catalyst comprises at least one of aluminum hydroxide, graphene oxide, and titanium dioxide.
9. A method for preparing a bipolar membrane for stable ion transport according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Preparation of gradient intermediate layer: Spinning solution A and spinning solution B are prepared and injected into microinjection pump 1 and microinjection pump 2 of a dual-channel electrospinning device respectively to prepare a multi-layer fiber structure. Microinjection pump 1 and microinjection pump 2 are controlled separately. The flow rates of microinjection pump 1 and microinjection pump 2 are dynamically adjusted so that the ratio of cation exchange resin to anion exchange resin in each layer of fiber gradually changes from 1:0 to 0:1 or from 0:1 to 1:
0. Meanwhile, during the spinning process of the gradient middle layer, a dispersion of a catalyst is continuously or periodically electrosprayed to obtain a gradient middle layer. (2) Preparation of bipolar membrane: The gradient middle layer is stacked together with the cation exchange membrane and the anion exchange membrane, wherein the cation exchange membrane is located on the side of the gradient middle layer with a high proportion of cation exchange resin, and the anion exchange membrane is located on the other side of the gradient middle layer, and then passed back and forth in a hot roller machine several times to obtain the bipolar membrane.
10. The method for preparing a bipolar membrane for stable ion transport according to claim 9, characterized in that: In step (1), the flow rate of the microinjection pump 1 is controlled between 0.0-1.0 mL / h or between 1.0-0.0 mL / h, and the flow rate of the microinjection pump 2 is synchronously controlled between 1.0-0 mL / h or between 0-1.0 mL / h.
Citation Information
Patent Citations
Bipolar film and preparation method thereof
CN1704151A
Bi pole membrane with low voltage of water disassociation, and prpearation method
CN1727058A