Material for constructing vegetation layer capable of absorbing air moisture and preparation method

By loading a polymer gel matrix with hydrophilic natural polymers and easily deliquescent salts, a vegetation layer that can absorb air moisture is constructed, which solves the problems of water self-sustainment and soil moisture regulation in arid environments, and improves the efficiency of plant growth and agricultural production. Water use efficiency.

CN118807625APending Publication Date: 2024-10-22CHENGDU UNIVERSITY OF TECHNOLOGY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411058912.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing technology cannot realize water self-sustaining and regulate soil moisture, and it is difficult to effectively utilize air moisture in arid and low-humidity environments, affecting agricultural production.

Method used

The polymer gel matrix loaded with hydrophilic natural polymers is combined with easily deliquescent salts to form a polymer aerogel, which enhances the hygroscopic performance and soil moisture self-sustaining ability, and builds a vegetation layer that can absorb air moisture.

Benefits of technology

It realizes the water demand for plant growth in arid environments, improves soil water adsorption and self-sustaining capabilities, reduces water management costs in agricultural production, and provides an economically feasible and ecologically sustainable solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807625A_ABST
    Figure CN118807625A_ABST
Patent Text Reader

Abstract

The invention discloses a material for constructing a vegetation layer capable of absorbing air moisture and a preparation method, and belongs to the technical field of environmental ecological restoration, the material comprises a polymer gel matrix and a hydrophilic natural polymer loaded on the polymer gel matrix; the gel comprises a polymer gel matrix, a deliquescent salt and a hydrophilic natural polymer matrix loaded on the polymer gel matrix, so that the absorption, transportation and storage of water and the loading of the deliquescent salt are facilitated, and the mechanical property of the gel can be enhanced by introducing the hydrophilic natural polymer. The salt easy to deliquesce is used as a moisture absorption component of the moisture absorption gel to collect water in the atmosphere, and the problems that in the prior art, water self-sustaining cannot be achieved, and soil moisture cannot be regulated and controlled are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental ecological restoration, and in particular to a material for constructing a vegetation layer capable of absorbing air moisture and a preparation method thereof. Background Art

[0002] Water is a fundamental environmental factor for agricultural food production. However, drylands account for more than 40% of the Earth's land area, including 45% of the world's agricultural land. Climate change and anthropogenic pollution have exacerbated desertification, posing a threat to agricultural production due to water shortages. Especially in arid regions, freeing crop cultivation from complex water supply chains will have a significant impact on reducing costs and provide obvious ecological advantages. This urgent need has prompted people to explore a new water resource - atmospheric water, which can be used without being restricted by geographical and hydrological conditions. Atmospheric water harvesting (AWH) technology realizes a passive method of obtaining water from the air. This technology does not require centralized water and electricity supply, thus bringing hope for energy sustainability in agriculture. Water management in the soil is also important to prevent water loss due to evaporation and drainage.

[0003] A Chinese patent with application number 201980032835.6 discloses a material and device for collecting water vapor, which comprises a deliquescent salt, a photothermal agent, and a polymer gel matrix containing a deliquescent salt and a photothermal agent. The inclusion of a photothermal agent in the material for collecting atmospheric water enables the material for collecting atmospheric water to generate heat under natural sunlight, which causes the material for collecting atmospheric water to be heated and evaporate the absorbed water vapor. The above scheme mainly realizes the water collection function by absorbing water and releasing water by increasing the temperature, and is mainly used for obtaining clean water. However, the demand for water for agricultural irrigation is huge, and clean water needs to be redistributed. If the function of directly regulating soil moisture can be used by air water collection technology, it is very important to achieve water self-sustaining capacity, and its application prospects are broad. Summary of the invention

[0004] The present invention provides a material and a preparation method for constructing a vegetation layer capable of absorbing moisture from the air, which solves the problem in the prior art that it is impossible to achieve self-sustaining moisture and regulate soil moisture.

[0005] In order to solve this technical problem, the present invention provides the following technical solution: A material for constructing a vegetation layer capable of absorbing moisture from the air, comprising: polymer gel matrix; and a hydrophilic natural polymer loaded on the polymer gel matrix; and deliquescent salts.

[0006] Preferably, the polymer gel matrix comprises at least one of poly(acrylic acid), poly(vinyl pyrrolidone), poly(acrylamide), poly(ethylene oxide), poly(vinyl alcohol), poly(2-hydroxyethyl vinyl ether) and poly(N-isopropylacrylamide).

[0007] Preferably, the hydrophilic natural polymer loaded on the polymer gel matrix is ​​selected from one or more of chitosan, starch or sodium alginate.

[0008] Preferably, the deliquescent salt is a chloride salt or a nitrate salt.

[0009] More preferably, the nitrate is zinc nitrate or calcium nitrate; the chloride is selected from any one of lithium chloride LiCl, calcium chloride CaCl2, magnesium chloride MgCl2, zinc chloride or ferric chloride FeCl3.

[0010] The present invention also provides a method for preparing the above-mentioned material for constructing a vegetation layer capable of absorbing air moisture, comprising: forming a polymer gel matrix loaded with hydrophilic natural polymers; Freeze-drying the polymer gel matrix loaded with hydrophilic natural polymers to form a polymer aerogel; and The polymer aerogel is immersed in a solution containing a deliquescent salt, and the polymer aerogel is taken out and dried to obtain the material for constructing a vegetation layer capable of absorbing moisture from the air.

[0011] Preferably, the forming of the polymer gel matrix loaded with hydrophilic natural polymers comprises: dissolving the hydrophilic natural polymers in a solvent to form a hydrophilic natural polymer solution; mixing the monomers of the polymer gel matrix with the hydrophilic natural polymer solution to dissolve the monomers to obtain a monomer mixture; A crosslinking agent and an initiator are added to the monomer mixture, and the mixture is stirred to react to form a polymer gel matrix loaded with hydrophilic natural polymers.

[0012] Preferably, the solvent is selected from an organic acid solution or water; preferably, the organic acid solution is selected from an acetic acid solution or a propionic acid solution; preferably, the monomer of the polymer gel matrix is ​​selected from acrylamide, N-isopropylacrylamide, acrylic acid, N-vinylpyrrolidone, ethylene oxide, vinyl acetate, 2-hydroxyethyl vinyl ether; preferably, the crosslinking agent is selected from N,N'-methyleneacrylamide MBA; preferably, the initiator is selected from potassium persulfate or ammonium persulfate.

[0013] Preferably, the freeze drying comprises: washing the polymer gel matrix with deionized water and soaking it to swell, then pre-freezing it at -20°C for 12 hours, and then continuing vacuum freeze drying for 48 hours until the sample is dry to form a polymer aerogel.

[0014] Preferably, the concentration of the deliquescent salt solution is 0.0125 g / mL-0.05 g / mL.

[0015] The present solution also provides a vegetation layer capable of absorbing moisture from the air, comprising the above-mentioned materials for constructing the vegetation layer capable of absorbing moisture from the air and vegetation soil; the dosage of the materials for constructing the vegetation layer capable of absorbing moisture from the air is 0.3%-2.4%.

[0016] Compared with the prior art, the present invention has the following advantages: Based on polymer gel, this scheme takes into account the economic cost of macro-quantity production and large-scale application and the limited sustainability of lithium resources. By loading biological molecules on the polymer gel matrix and loading hygroscopic salts such as CaCl2 to achieve hygroscopic dynamic function, this scheme constructs a biopolymer gel with excellent performance, environmental friendliness, economic feasibility, and ecological sustainability, solving the water demand for plant growth in arid and low-humidity desert environments. The hydrophilic natural polymer matrix loaded on the polymer gel matrix in this solution not only facilitates the absorption, transportation, storage of water and the loading of hygroscopic salts, but also enhances the water storage capacity and improves the mechanical properties of the gel.

[0017] The freeze-dried polymer gel matrix loaded with hydrophilic natural polymers is immersed in a deliquescent salt solution. The ions in the solution react with the carbonyl groups on the aerogel skeleton. In addition, a large amount of deliquescent salt is distributed in the pores and surface of the aerogel. Due to the coverage of the salt, the contact area between the hygroscopic salt and the water molecules in the air is increased, which is beneficial to improving its hygroscopic properties.

[0018] The vegetation layer constructed by the materials of this scheme and the soil has a positive effect on plant growth and development under drought stress, and the gel material enhances the soil's ability to absorb and sustain moisture. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings: Figure 1 This is a physical picture of the calcium-based aerogel PAM-CS-CaCl2 prepared in Example 1 of the present invention; Figure 2 The scanning electron microscope images of the aerogel matrix and calcium-based aerogel prepared in the present invention are shown in FIG. Figure 2 a- Figure 2 d is a scanning electron microscopy image of the PAM-CS matrix of Comparative Example 1; Figure 2 e- Figure 2h is a scanning electron microscope image of PAM-CS-CaCl2 of Example 1; Figure 3 The storage modulus (G′) and loss modulus (G″) of the PAM of Comparative Example 2 and the PAM-CS hydrogel of Comparative Example 1; Figure 4 is the dynamic contact angle of the PAM-CS matrix cross section; Figure 5 This is the Raman spectrum when the adsorption capacity of PAM-CS-CaCl2 is 2 g / g; Figure 6 (a) T2 spectra of calcium-based aerogel-sand with different doping amounts; Figure 6 (b) Filling pore size distribution of calcium-based aerogel-sand with different dosages; Figure 6 (c) NMR imaging of soil samples with different calcium-based aerogel dosages; Figure 7 Effects of different dosages of PAM-CS-CaCl2 on plant germination potential (a) and germination rate (b); Figure 8 The effect of aerogels with different CaCl2 concentrations on plant height; Fig. 9 The effect of aerogels with different CaCl2 concentrations on the water content of plant leaves; Fig.10 The effect of aerogels with different CaCl2 concentrations on plant weight; Fig.11 The effect of aerogels with different CaCl2 concentrations on the root-shoot ratio of plants; Fig.12 The effect of aerogels with different CaCl2 concentrations on plant biomass; Fig.13 (a) Effects of different aerogel dosages on plant growth (16 days); Fig.13 (b) Effects of aerogels with different CaCl2 concentrations on the survival days of plants; Fig.14 The hygroscopic properties of PAM-CS matrix and PAM-CS-CaCl2 at 90% RH and 25°C; Fig.15 (a) Moisture absorption curves of PAM-CS-CaCl2-sand with different dosages at 90% RH and 25°C; Fig.15 (b) Water retention curves of PAM-CS-CaCl2-sand and sand at RH = 20% and 40 °C; Fig.16 (a) is the temperature and relative humidity curve under natural conditions; Fig.16(b) is the moisture maintenance curve of saturated PAM-CS and PAM-CS-CaCl2 aerogels (under natural conditions); Fig.16 (c) The morphological changes of PAM-CS and PAM-CS-CaCl2 aerogels under natural release conditions; Fig.17 (a) is the growth status of plants after 10 days of drought stress; Fig.17 (b) Surface soil moisture after 10 days of drought stress; Fig.17 (c) Survival rate of plants without irrigation for 20 days under different aerogel treatments; Fig.18 (a) Moisture absorption properties of sand in an environment of 90% RH and 25°C at different aerogel dosages; Fig.18 (b) Fig.18 (a) PFO model fitting results; Fig.19 (a) Hygroscopic properties of silty loess in an environment of 90% RH and 25°C with different aerogel dosages; Fig.19 (b) Fig.18 (a) PFO model fitting results; Fig. 20 (a) Hygroscopic properties of yellow clay in an environment of 90% RH and 25°C at different aerogel dosages; Fig. 20 (b) Fig.18 (a) PFO model fitting results; DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The illustrative embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0021] The research of the prior art generally focuses on the water retention or water absorption performance of the material to achieve the water collection function, but cannot achieve the active air water collection capacity and the function of regulating soil moisture. This scheme is based on the biopolymer gel developed in the early stage, and is based on solving the water demand for plant growth in arid and low-humidity environments. Taking into account the economic cost and resource sustainability limitations of macro-quantity production and large-scale application, the inventor of this scheme has found that by using the biopolymer gel matrix to load hygroscopic salts, the hygroscopic dynamic function can be achieved, and a calcium-based biopolymer gel with excellent performance, environmental friendliness, economic feasibility, and ecological sustainability can be constructed. By studying the functional mechanism of the modified soil moisture regulation effect, it is found that the material of this scheme has a positive effect on plant growth and development under drought stress. The aerogel material has excellent soil moisture self-sustaining capacity and soil moisture regulation engineering. The following is a specific description of the implementation method of this application.

[0022] The method for preparing the material for constructing a vegetation layer capable of absorbing air moisture provided in the present scheme comprises: forming a polymer gel matrix loaded with hydrophilic natural polymers; Freeze-drying the polymer gel matrix loaded with hydrophilic natural polymers to form a polymer aerogel; and The polymer aerogel is immersed in a solution containing a deliquescent salt, and the polymer aerogel is taken out and dried to obtain the material for constructing a vegetation layer capable of absorbing moisture from the air.

[0023] In this solution, the hydrophilic natural polymer matrix loaded on the polymer gel matrix is ​​not only beneficial to the transportation and storage of water and the loading of CaCl2, but also the introduction of the hydrophilic natural polymer can enhance the mechanical properties of the gel.

[0024] The freeze-dried polymer gel matrix loaded with hydrophilic natural polymers is immersed in a deliquescent salt solution. The ions in the solution react with the carbonyl groups on the aerogel skeleton. In addition, a large amount of deliquescent salt is distributed in the pores and surface of the aerogel. Due to the coverage of the salt, the contact area between the hygroscopic salt and the water molecules in the air is increased, which is beneficial to improving its hygroscopic properties.

[0025] In the embodiment shown, the polymer gel matrix comprises poly(acrylamide), but the polymer gel matrix can comprise at least one of poly(acrylic acid), poly(vinyl pyrrolidone), poly(ethylene oxide), poly(vinyl alcohol), poly(2-hydroxyethyl vinyl ether), and poly(N-isopropylacrylamide).

[0026] In some embodiments, the hydrophilic natural polymer loaded on the polymer gel matrix is ​​selected from one or more of chitosan, starch or sodium alginate.

[0027] The introduction of hydrophilic natural polymers can not only enhance the mechanical properties of the gel, but also make the aerogel matrix have better hydrophilicity, which is conducive to the absorption and storage of liquid water.

[0028] In some embodiments, the deliquescent salt is a chloride salt or a nitrate salt. The nitrate salt is zinc nitrate or calcium nitrate; the chloride salt is selected from any one of lithium chloride LiCl, calcium chloride CaCl2, magnesium chloride MgCl2, zinc chloride or iron chloride FeCl3.

[0029] Deliquescent salts such as CaCl2 play a major role in the atmospheric water harvesting performance as the hygroscopic component of hygroscopic aerogels.

[0030] In some embodiments, the forming of a polymer gel matrix loaded with hydrophilic natural polymers comprises: Dissolving a hydrophilic natural polymer in a solvent to form a hydrophilic natural polymer solution; Mixing the monomers of the polymer gel matrix with the hydrophilic natural polymer solution to dissolve the monomers to obtain a monomer mixture; Adding a crosslinking agent and an initiator to the monomer mixture, stirring and reacting to form a polymer gel matrix loaded with hydrophilic natural polymers; Polymer gel matrices loaded with hydrophilic natural polymers such as PAM-CS serve as aerogel skeletons loaded with hygroscopic salts, providing channels and carriers for the transmission and storage of liquid water.

[0031] In some embodiments, the solvent is selected from an organic acid solution or water; the organic acid solution is selected from an acetic acid solution or a propionic acid solution; the monomer of the polymer gel matrix is ​​selected from acrylamide; the linker is selected from N,N'-methylene acrylamide MBA; the initiator is selected from potassium persulfate or ammonium persulfate; the monomer of the polymer gel matrix can also be selected from at least one of N-isopropylacrylamide, acrylic acid, N-vinyl pyrrolidone, ethylene oxide, vinyl acetate and 2-hydroxyethyl vinyl ether.

[0032] In some embodiments, the freeze-drying comprises: washing the polymer gel matrix with deionized water and soaking it to swell, then freezing it in a -20°C refrigerator for 12 hours, and continuing freeze-drying for 48 hours until the sample is dry to form a polymer aerogel.

[0033] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially. Example 1

[0034] Weigh 2g chitosan (CS) and dissolve it in 100mL acetic acid solution (volume fraction 2.5%) to prepare CS aqueous solution (w=2%); weigh 0.5g acrylamide (AM) and ultrasonicate it in 5mL CS solution for 1min to fully dissolve the monomer, then add 0.4mL 3.8mg / mL crosslinker N,N'-methylene acrylamide (MBA) and 0.2mL 50mg / mL initiator potassium persulfate (KPS) in sequence, stir gently and ultrasonicate it for 2min, react at 70℃ for 2h to form a gel, rinse the above hydrogel with a large amount of deionized water to remove the unreacted monomer, and soak it for 72h, changing the water every 8h to allow it to swell fully. After being placed in a -20 °C refrigerator for 12 h, the sample was freeze-dried for 48 h (until the sample was dry); the freeze-dried aerogel was immersed in a CaCl2 solution with a concentration of 0.05 g / mL, taken out after 24 h, and dried in an 80 °C drying oven for 72 h to obtain PAM-CS-CaCl2 aerogel. Example 2

[0035] The difference between this example and Example 1 is that a CaCl2 solution with a concentration of 0.0125 g / mL is used instead of the CaCl2 solution with a concentration of 0.05 g / mL in Example 1 for the experiment, and other experimental conditions remain unchanged. Example 3

[0036] The difference between this example and Example 1 is that a CaCl2 solution with a concentration of 0.025 g / mL is used instead of the CaCl2 solution with a concentration of 0.05 g / mL in Example 1 for the experiment, and other experimental conditions remain unchanged. Example 4

[0037] The difference between this embodiment and embodiment 1 is that a CaCl2 solution with a concentration of 0.1 g / mL is used instead of the CaCl2 solution with a concentration of 0.05 g / mL in embodiment 1 for the experiment, and other experimental conditions remain unchanged. Example 5

[0038] Weigh 2 g of sodium alginate (SA) and dissolve it in 100 mL of water (volume fraction of 2.5%) to prepare a sodium alginate aqueous solution (w=2%); weigh 0.5 g of N-isopropylacrylamide (NIPAM) and ultrasonicate it in 5 mL of sodium alginate solution for 1 min to fully dissolve the monomer, then add 0.4 mL of 3.8 mg / mL of cross-linking agent N,N'-methyleneacrylamide (MBA) and 0.2 mL of 50 mg / mL of initiator potassium persulfate (KPS) in turn, stir gently and ultrasonicate it for 2 min, react at 70°C for 2 h to form a gel, rinse the above hydrogel with a large amount of deionized water to remove unreacted monomers, and soak it for 72 h, changing the water every 8 h to allow it to fully swell. After being placed in a -20°C refrigerator for 12 h, the sample was freeze-dried for 48 h (until the sample was dry); the freeze-dried aerogel was immersed in CaCl2 solutions of different concentrations, taken out after 24 h and placed in an 80°C drying oven for 72 h to obtain NIPAM-SA-CaCl2 aerogel. Example 6

[0039] Weigh 2g starch and dissolve it in 100mL aqueous solution to prepare starch aqueous solution (w=2%); weigh 0.5g acrylamide (AM) and ultrasonicate it in 5mL sodium alginate solution for 1min to fully dissolve the monomer, then add 0.4mL of 3.8mg / mL crosslinker N,N'-methylene acrylamide (MBA) and 0.2mL of 50mg / mL initiator potassium persulfate (KPS) in turn, stir gently and ultrasonicate for 2min, react at 70℃ for 2h to form gel, rinse the above hydrogel with a large amount of deionized water to remove unreacted monomers, and soak it for 72h, changing the water every 8h to make it fully swell. After freezing in a -20℃ refrigerator for 12h, freeze-dry it for 48h (until the sample is dry); soak the freeze-dried aerogel in CaCl2 solution of different concentrations, take it out after 24h and dry it in an 80℃ drying oven for 72h to obtain PAM-amylum-CaCl2 aerogel.

[0040] Comparative Example 1 The difference between this comparative example and Example 1 is that no deliquescent salt is loaded. The specific preparation process is as follows: Weigh 2g chitosan (CS) and dissolve it in 100mL acetic acid solution (volume fraction 2.5%) to prepare CS aqueous solution (w=2%); weigh 0.5g acrylamide (AM) and ultrasonicate for 1min in 5mL CS solution to fully dissolve the monomer, then add 0.4mL of 3.8mg / mL crosslinker N,N'-methylene acrylamide (MBA) and 0.2mL of 50mg / mL initiator potassium persulfate (KPS) in turn, stir gently and ultrasonicate for 2min, react at 70℃ for 2h to form gel, rinse the above hydrogel with a large amount of deionized water to remove unreacted monomers, and soak for 72h, changing the water every 8h to make it fully swell. Place it in a -20℃ refrigerator for 12h, and freeze-dry it for 48h (until the sample is dry); soak the freeze-dried aerogel in deionized water solution, take it out after 24h and place it in an 80℃ drying oven for 72h to dry it to obtain PAM-CS gel matrix.

[0041] Comparative Example 2 The difference between Comparative Example 2 and Comparative Example 1 is that chitosan is not added; the preparation process is as follows: Weigh 0.5g acrylamide (AM) in 5mL aqueous solution and ultrasonicate for 1min to fully dissolve the monomer, then add 0.4mL of 3.8mg / mL crosslinker N,N'-methylene acrylamide (MBA) and 0.2mL of 50mg / mL initiator potassium persulfate (KPS), stir gently and ultrasonicate for 2min, react at 70℃ for 2h to form gel, rinse the hydrogel with a large amount of deionized water to remove unreacted monomer, and soak for 72h, changing the water every 8h to make it fully swell. Place it in a -20℃ refrigerator for 12h, and freeze-dry it for 48h (until the sample is dry); soak the freeze-dried aerogel in deionized water solution, take it out after 24h and place it in an 80℃ drying oven for 72h to dry it to obtain PAM gel.

[0042] Application Test Example 1 In order to study the effect of aerogel on the pore size distribution of vegetation layer soil, nuclear magnetic resonance (NMR) was used to study the change of different aerogel dosages on the pore microstructure of sand over time. The calcium-based aerogel prepared in Example 1 was uniformly mixed with sand at different dosages (0%, 0.3%, 0.6%, 1.2%, 2.4% and 5%, calculated by the weight of dry sand), deionized water was added, and stirred to form a uniform aerogel-sand mixture. The mixture was then transferred to a Φ60×20mm mold and finally placed in a vacuum saturated cylinder for saturation overnight. Saturated samples are required in these tests because only the pores are completely filled with water; the signals detected by nuclear magnetic resonance can characterize the pore volume and size of the sample. The sampling process was started, and the CPMG-loose soil sequence was selected. The entire T2 signal measurement process lasted for 2-3 min, and the size of the polymer-filled pores was obtained by inversion of the nuclear magnetic resonance signal. And the NMR imaging was obtained by nuclear magnetic resonance imaging.

[0043] In porous media, transverse relaxation time (T2) and signal amplitude are two key parameters, which reflect the different microstructures of water or other materials containing hydrogen protons. T2 can be expressed as formula (1): ; In formula (1): T 2b ——Volume relaxation time; T 2d ——Diffusion relaxation time; T 2s ——surface relaxation time; ρ2——surface relaxation rate; S ——pore surface area; V ——pore volume; Among them, since the volume relaxation and diffusion relaxation have little effect on the total relaxation time under the action of uniform magnetic field, the T 2b and T 2d Therefore, the surface relaxation time (T2) is determined by the pore surface area (S), pore volume (V) and surface relaxation rate (ρ2).

[0044] Assuming that the pore structure of the soil sample is spherical, equation (1) can be simplified to equation (2): ; Where, R is the pore radius; Application Test Example 2 Since the concentration of the hygroscopic component CaCl2 has a great influence on the hygroscopic properties of calcium-based aerogels and plant growth, the aerogels prepared in Examples 1-4 were ground and uniformly mixed with sand according to different aerogel dosages (0%, 0.3%, 0.6%, 1.2%, and 2.4%, respectively), and the CK group with a dosage of 0% was all natural sand.

[0045] The plant planted was ryegrass of Dongmu 70. To break the dormancy of seeds, the seeds were first soaked in warm water for 24 h and the water was changed every 5 h. 16 full and uniform seeds were selected for each pot and sprinkled 1.5 cm below the soil surface. After covering the soil, the soil and seeds were sprayed with a watering can. The amount of water for each group of pots was consistent, and the seeds were not exposed to the soil surface. The size of the flowerpot was 9.5 cm high, the upper diameter was 7 cm, and the lower diameter was 5 cm. Three parallel tests were conducted in each group of experiments. During the plant cultivation process, water was poured once every 3 days, 50 mL each time. After 2 waterings, drought stress treatment was started (no more maintenance), and the pots were placed in a dry plant culture room (relative humidity 20~30% RH, 23~25℃) to simulate a drought environment.

[0046] (1) Determination of plant germination rate The number of seeds that germinated was recorded 2-5 days after sowing. The germination rate was the ratio of the number of seeds that germinated to the number of seeds sown.

[0047] (2) Determination of plant height and root length Take the plant out of the pot completely and rinse it carefully with water. Use a ruler to measure the height and root length of the plant. The height above the rhizome boundary is the plant height, and the length of the plant root system below the rhizome boundary is the plant length. Repeat each measurement 3 times.

[0048] (3) Determination of water content of plant leaves Leaf moisture content is a method to evaluate the water status of plants. The growth and development of plants are affected by the moisture in the environment, so the assessment of the water status of plants is very important. After 5 days of drought stress, the leaves of the plants in the plant culture room were taken out and immediately weighed with a 1 / 10,000 analytical balance, recorded as m1, and 3 parallel tests were performed in each group. Then they were placed in a 105°C oven for 15 minutes, and then the temperature was adjusted to 80°C to dry until constant weight, and the weight was recorded as m2. The leaf moisture content w (%) was calculated as follows: ; (4) Determination of plant fresh weight After 5 days of drought stress, the plants were completely removed from the pots, and the soil and aerogel attached to the roots were washed off with clean water. After drying with a paper towel, the plants were weighed with a 1 / 10,000 balance, and each set of measurements was repeated at least three times.

[0049] (5) Determination of plant root-to-shoot ratio The root-to-shoot ratio can reflect the growth status of plants and the different effects of environmental conditions on the growth of the aboveground and underground parts. The root-to-shoot ratio is the ratio of the dry weight or fresh weight of the underground part of the plant to the aboveground part. After 5 days of drought stress, the dry weight of the underground biomass of the plant is compared with the dry weight of the aboveground biomass to obtain the root-to-shoot ratio.

[0050] (6) Determination of plant biomass After 5 days of drought stress, the plants were completely removed from the pots, the roots were carefully cleaned and dried with paper towels. The plants were cut at the boundary of the rhizome with scissors, the above-ground and underground parts were marked and placed in a 105°C oven for 15 minutes, and then the temperature was adjusted to 80°C and dried to constant weight. Finally, the above-ground and underground parts were weighed with a 1 / 10,000 scale. The total biomass of the plant is the sum of the above-ground biomass and the underground biomass.

[0051] (7) Determination of plant survival time The potted plants were placed in a dry plant culture room (about 20% RH, 25°C) to simulate a drought environment. When the seedlings grew to a certain height, they were no longer watered and maintained without management. The growth of the plants was observed and recorded every day until all the plants died.

[0052] Application Test Example 3 The calcium-based aerogel prepared in Example 1 and the material prepared in Comparative Example 1 were tested for their soil moisture self-sustaining capacity.

[0053] (1) Hygroscopicity test of calcium-based aerogel PAM-CS-CaCl2 The constant temperature and humidity conditions in the water adsorption test are provided by a constant temperature and humidity chamber. In order to allow the aerogel to fully contact the humid air, it is placed on a suspended stainless steel net and placed in a constant temperature and humidity chamber with different relative humidity. During the moisture absorption process, the aerogel is weighed once every hour with an analytical balance to record the mass change of the aerogel. The adsorption capacity is calculated as follows: ; Among them, m i ——The total mass of aerogel after moisture absorption at different times, m0——initial dry weight of aerogel.

[0054] (2) Moisture absorption and desorption performance test of calcium-based aerogel-sand The adsorption performance test of calcium-based aerogel-sand was carried out in a constant temperature and humidity chamber. The aerogel was ground into uniform fine particles and then evenly mixed with dry sand. The aerogel dosage was set to 0%, 0.3%, 0.6%, 1.2%, and 2.4%, respectively. It was placed in a constant temperature and humidity chamber at 90% RH and 25°C. During the hydration process, the weight of the sample was tracked with an analytical balance until the adsorption capacity reached equilibrium (no weight change within 30 minutes). The adsorption curve can be obtained by the change of sample weight over time.

[0055] The adsorption saturated aerogel was placed in an oven at 40°C and 20% relative humidity for release testing. During the dehydration process, the weight of the sample was tracked with an analytical balance until the moisture content reached equilibrium (no weight change within 30 minutes). The water release curve can be obtained by the change in sample weight over time.

[0056] (3) Water holding performance test of adsorption saturated aerogel matrices PAM-CS and PAM-CS-CaCl2 under natural conditions In order to verify that the function of calcium-based aerogel in regulating the vegetation layer is not only the water retention of the PAM-CS matrix, but also the water-holding effect of PAM-CS-CaCl2 due to its water collection performance, the two saturated aerogels were placed under natural conditions, and their weight changes and aerogel morphology changes were recorded, and the relative humidity and temperature under natural conditions were recorded. The adsorption method was completed by solution immersion. Since the PAM-CS matrix has no adsorption capacity for air, it was placed in deionized water to absorb water and swell until adsorption equilibrium was reached; the calcium-based aerogel PAM-CS-CaCl2 was immersed in a 0.05 g / mL PAM-CS-CaCl2 solution until equilibrium was reached, and finally the water on the surface of the gel was wiped dry with filter paper for standby use.

[0057] (4) Pot test of aerogel matrix PAM-CS and PAM-CS-CaCl2 To further verify the water-holding effect of PAM-CS-CaCl2 in regulating the function of the vegetation layer, matrix aerogel and calcium-based aerogel vegetation layers were constructed, and the characteristic indicators of plant growth in the reconstructed soil were monitored and analyzed. Sandy soil was evenly mixed with ground PAM-CS and PAM-CS-CaCl2 to plant Dongmu 70 ryegrass. The aerogel dosage was 0.6%. The blank group (CK) was planted in pure sandy soil. Three parallel experiments were set up. During the plant growth process, the potted plants were placed indoors, and the growth of the plants, such as survival time, was observed and recorded.

[0058] Application Test Example 4 The moisture absorption performance of the calcium-based aerogel PAM-CS-CaCl2 prepared in Example 1 was tested on soils of different textures (sand, silt, clay).

[0059] The constant temperature and humidity conditions in the water vapor adsorption test of soils with different textures were provided by a constant temperature and humidity chamber. 6g of soils with different textures were weighed separately: desert sand (sand soil) from Wuwei, Gansu, silty loess from Yan'an, Shaanxi, and yellow clay from Chengdu, Sichuan. Calcium-based aerogel PAM-CS-CaCl2 powder was added at 0.4%, 0.8%, 1.6%, and 3.2% of the dry soil mass, and fully stirred. The modified soil was placed on a watch dish and placed in a constant temperature and humidity chamber with a relative humidity of 90%. The soil was weighed once every hour with an analytical balance during the moisture absorption process, and the mass change of the aerogel was recorded.

[0060] The PFO model (pseudo first-order model) was used to fit the adsorption kinetics curve to obtain the adsorption rate constant, as shown in the following formula 5: , Among them, q t ——Modified soil moisture content at time t, q e ——Modified soil moisture content at equilibrium time, k1 – adsorption rate constant.

[0061] The actual picture of the calcium-based aerogel PAM-CS-CaCl2 prepared in Example 1 is as follows Figure 1 As shown, it is shown that the aerogel is successfully prepared in Example 1 of this scheme; In order to observe the surface morphology and pore structure of the aerogel, the cross-sections of the freeze-dried PAM-CS obtained in Comparative Example 1 and the PAM-CS-CaCl2 in Example 1 were subjected to scanning electron microscopy (SEM) analysis. Figure 2 adIt can be seen that the freeze-dried PAM-CS matrix aerogel presents a loose and porous structure, the inner wall of the aerogel is smooth, and the pores are fluffy and distinct, which is conducive to the transportation and storage of water and the loading of CaCl2. Figure 2 eh, the pore structure of PAM-CS-CaCl2 has changed significantly, which may be due to the collapse of the pores caused by high-temperature drying after hygroscopic salt loading; however, it can also be observed that the pore wall thickness has increased, which has strengthened the strength of the aerogel skeleton. This is because the freeze-dried PAM-CS is immersed in a CaCl2 solution, and the calcium ions in the solution react with the carbonyl groups on the aerogel skeleton. In addition, a large amount of CaCl2 is distributed in the aerogel pores and surface, which Figure 2 It can be observed that the surface of the pore wall of PAM-CS-CaCl2 aerogel presents clear texture, which is due to the coverage of CaCl2; this increases the contact area between the hygroscopic salt and the water molecules in the air, which is beneficial to improving its hygroscopic performance.

[0062] The dynamic rheological properties of the PAM gel of Comparative Example 2 and the PAM-CS gel of Comparative Example 1 (2.5 cm in diameter and 1 cm in height) were tested using a rheometer (MCR102, Anton Paar, Germany). The frequency scanning range was 0.1–100 rad / s, the gap was 2.757 mm, and the temperature was 20.54°C. As a viscoelastic material, the gel has the characteristics of energy storage and dissipation. The corresponding storage modulus (G′) and loss modulus (G″) can be measured by the rheometer, thereby revealing the structural differences of the hydrogel. In order to prove the coagulation effect of PAM and chitosan, PAM hydrogel was prepared in Comparative Example 2 as a blank sample. As shown in FIG. Figure 3As shown in the figure, from the rheological data of the two gels, G′ has higher values ​​than G″, which proves the stable cross-linked skeleton of these hydrogels. Storage modulus, as one of the important indicators of mechanical properties, reflects the stiffness and elastic deformation ability of the material. Compared with PAM, PAM-CS has higher G′, indicating that the introduction of chitosan enhances the mechanical properties of the gel.

[0063] Take a smooth aerogel sample, place it on the JY-82 contact angle test platform, adjust the table, use the automatic titration system of the equipment to drop 16ul of water, take test photos, and the time interval between each photo is 50ms. Use the high-volume method to measure the contact angle. When the droplet reaches equilibrium on the surface of the solid, the angle between the gas-liquid interface and the liquid-solid interface at the junction of the gas, liquid and solid phases is the contact angle, which can be used to evaluate the wettability of the contact surface between the solid and the liquid; the hydrophilicity and hydrophobicity of the aerogel matrix are analyzed by the contact angle. Figure 4 The dynamic contact angle images of the freeze-dried PAM-CS matrix were taken at 0s, 60s, 90s, and 110s. Figure 4 It can be observed that the droplet is completely absorbed by the matrix after falling 110, and the contact angle is 0. This shows that the aerogel PAM-CS matrix has good hydrophilicity, which is conducive to the absorption and storage of liquid water.

[0064] The calcium-based aerogel was placed in a constant temperature and humidity chamber at 90% RH and 25°C to absorb moisture. When the adsorption capacity reached 2g / g, the alpha300R Raman spectrometer produced by WITec of Germany was used to characterize the state of adsorbed water in the aerogel. The laser wavelength was 532nm, and the test wave number range was 2500-4000cm -1 , Single spectrum test conditions: laser energy 50mW, 600g / mm grating, Olympus 20x objective lens (Olympus 20x / 0.25), integration time 35s, accumulation times 6 times. Figure 5 As shown in the figure, the Raman spectrum of PAM-CS-CaCl2 after adsorption (water content is 2g / g) is at 2928cm -1 There is a small peak nearby corresponding to CH at 3430 cm -1 There is a peak nearby corresponding to -OH, which is fitted into 4 peaks. -1 、3401cm -1 The peak is free water, at 3515cm -1 、3630cm -1 The peak corresponds to intermediate water, and the results confirm the existence of intermediate water in PAM-CS-CaCl2, which is beneficial to the desorption of water.

[0065] In order to quantitatively detect the effect of aerogel on the porosity characteristics of sand, the sample was tested by nuclear magnetic resonance using Test Example 1. Since there is a linear relationship between the total signal intensity of NMR and the pore size distribution, the T2 spectrum distribution curve can be converted into a pore size distribution curve by calculation. The T2 spectra of samples with different calcium-based aerogel dosages and the aerogel-filled pore size distribution curves are shown in the figure. By observation, according to the distribution characteristics of the characteristic peaks, it can be roughly divided into three regions, corresponding to micropores, mesopores and macropores. The pore types of this sand are mainly micropores and mesopores. Figure 6 b shows the proportions of various pore types. Figure 6 As the content of calcium-based aerogel increases in a, the amplitude and peak area of ​​the characteristic peak in the T2 spectrum gradually decrease, such as Figure 6 b. As the calcium-based aerogel content increases from 0% to 5%, the total porosity decreases from 37.64% to 13.19%, which indicates that the pore size of the calcium-based aerogel-sand becomes smaller, and the number and volume of pores decrease. The distribution of each pore type is as follows: Compared with pure sand, with the addition of calcium-based aerogel, the macropore characteristic peak completely disappears, and the proportion decreases from 0.88% to 0%, because macropores are more easily filled by aerogel. Figure 6In a, the calcium-based aerogel content increased from 0.0% to 0.6%, and the characteristic peak of mesopores changed from a single peak of pure sand to a double peak, which means that the amount of calcium-based aerogel adhering to the surface of sand particles increased, and more peaks and better ordering appeared. The amplitude of the characteristic peak decreased, the peak area decreased, and the relative content of mesopores decreased from 36.76% to 24.73%. However, as the calcium-based aerogel content increased from 1.2% to 5.0%, the characteristic peak of sand returned to a single characteristic peak, which may be because the calcium-based aerogel had limited sites adhering to the surface of sand particles. Since too much aerogel produced stronger swelling sites after absorbing water, part of the soil structure may be destroyed. At this time, the relative content of mesopores decreased from 21.03% to 12.87%. The characteristic peak amplitude and initial and final relaxation time of the small pores in the calcium-based aerogel-sand soil are larger than those in the bare sand. As the calcium-based aerogel content increases, the characteristic peak moves to the left. When the calcium-based aerogel content increases from 0% to 1.2%, the proportion of micropores increases from 0.11% to 0.63%; as the calcium-based aerogel content increases from 1.2% to 5.0%, the proportion of micropores decreases from 0.63% to 0.32%. The increase in micropores first may be because the calcium-based aerogel with a lower content absorbs a large amount of water vapor from the air and expands in volume. During the expansion process, the surrounding small pores are compressed into micropores, increasing the micropore content and improving the initial structure of the soil. As the soil moisture gradually decreases, the moisture in the calcium-based aerogel is slowly released under the adsorption capacity of the soil particle surface to keep the soil moist. When the soil moisture is sufficient, the calcium-based aerogel still absorbs excess free water and stores it in its molecular structure. As the calcium-based aerogel dosage increases, the proportion of micropores decreases because the swelling of the aerogel after absorbing water causes more micropores to be squeezed. Figure 6 c is the saturated calcium-based aerogel-sand NMR imaging obtained from the nuclear magnetic resonance analyzer. The fluorescent bright spots in the picture represent the water content. The increase in brightness indicates the increase in water content. It also represents the high porosity, strong connectivity and uniform distribution of natural sand. As the calcium-based aerogel dosage increases, the overall imaging becomes darker and the number of bright spots decreases significantly, which means that the total pores of the calcium-based aerogel are significantly reduced. On the one hand, calcium-based aerogel can significantly reduce the porosity and permeability of natural sand, making the natural sand more compact, improving the water retention of sand and slowing down water loss; on the other hand, calcium-based aerogel continuously absorbs water from the air and increases the effective water content in the sand. Compared with the calcium-based aerogel content of 2.4%, due to the high dosage of 5%, the density of the aerogel in the sand is too large, and after absorbing water and swelling, they contact each other to form a larger agglomerated hydrogel. This is why there are still a small number of bright spots in the 5% dosage sample.

[0066] like Figure 7It can be seen that with the increase of the amount of aerogel PAM-CS-CaCl2, the germination rate of ryegrass showed a decreasing trend. When the amount of aerogel added was 0.3%, the germination rate reached 96%, which was 12.67% higher than that of the CK group. The germination rate of the plant with an aerogel addition of 0.6% was equivalent to that of the CK, while the germination rate of the plant with an aerogel addition of 2.4% was only 54.17%, and the plant grew short and showed a state of dehydration. This may be due to salt stress caused by excessive CaCl2. For plant buds, excessive Cl - It will inhibit its growth. Therefore, 0.3% and 0.6% aerogel additions were selected for subsequent tests.

[0067] Considering the great influence of CaCl2 on plants, the application test example 2 explores the influence of different CaCl2 concentrations on plant growth indicators (plant height, root length, leaf moisture content, biomass, etc.), and then selects the aerogel with the best CaCl2 concentration for vegetation layer construction. Figure 8 The figure shows the effect of aerogels with different CaCl2 concentrations on plant height. In the early growth stage of ryegrass, plants with high concentrations of CaCl2 grew slowly. With the increase of CaCl2 concentration, the height of plants with both dosages increased first and then decreased, and both reached the maximum height at a concentration of 0.05g / mL. With the increase of CaCl2 concentration in aerogel, the height of plants with a concentration of 0.1g / mL decreased compared with the CK group; and the height of plants with a dosage of 0.3% was higher than that of plants with a dosage of 0.6%. The leaves and stems of plants in the 0.6% dosage group and the 0.1g / mL concentration group were purple in color, while the plants in the low concentration and low dosage groups were obviously light green. This is because the higher salt concentration causes "salt stress" to the plants, which will limit the growth of the plants to a certain extent.

[0068] The leaf moisture content can reflect the water status of plants. By measuring the leaf moisture content of plants, the drought resistance and adaptability of plants can be evaluated. On the fifth day without maintenance management, the leaf moisture content is as follows. Fig. 9 As shown in the figure, the leaf moisture content of the CK group was 59.68% and 57.77%, respectively, while the leaf moisture content of the aerogel vegetation layer plants increased with the increase of CaCl2 concentration. The leaf moisture content of the 0.6% doping increased first and then decreased with the increase of CaCl2 concentration, and reached the highest leaf moisture content of 85.21% at a salt concentration of 0.05g / mL. According to the leaf moisture content, the drought resistance of plants under different salt concentrations of aerogel was ranked: blank group <C 0.0125g / mL < C 0.025g / mL < C 0.05g / mL ≤ C 0.01g / mL。 Considering the cost and the impact of salt on soil and plants, aerogels with a salt concentration of 0.05 g / mL are preferred.

[0069] like Fig.10 The effect of different treatments on plant weight after 5 days of drought stress. The plant weight of the treatment with aerogel added was significantly increased compared with CK, and the plant weight was the highest when the salt concentration was 0.05g / mL. This shows that calcium-based aerogel acts as a "water pump" to continuously supply water to plants, promote plant growth, and increase plant weight.

[0070] The root-to-shoot ratio is shown in Fig.11 As shown in the figure, the root-to-crown ratio of the CK group is the largest, and the root-to-crown ratio of the plants treated with aerogel first decreases and then increases with the increase of salt concentration, and the root-to-crown ratio of the CK group is larger than that of the experimental group. This is because the root-to-crown ratio will increase when the soil moisture is insufficient.

[0071] like Fig.12 As shown in the figure, the biomass of the plants has a similar trend to that of the fresh weight, which increases first and then decreases with the increase of salt concentration. Under the same conditions, the biomass of the aerogel with a 0.3% aerogel dosage is higher than that of the 0.6% aerogel. The biomass of the aerogel treatments with salt concentrations of 0.0125 g / mL, 0.025 g / mL, 0.05 g / mL, and 0.1 g / mL are 173.31 g / cm 2 , 195.63 g / cm 2 , 257.07 g / cm 2 , 206.29 g / cm 2 , which were 39.59%, 57.56%, 107.05% and 66.20% higher than those of CK, respectively.

[0072] like Fig.13 a. On the 16th day, the plants in the CK group all withered due to lack of water, while the experimental group treated with aerogel grew vigorously. The vitality of the plants treated with 0.6% addition was higher than that of the plants treated with 0.3% addition. The higher the salt concentration, the better the plant condition.

[0073] like Fig.13 As shown in Figure b, the results of plant survival time show that within this range of salt concentration and aerogel dosage, as the salt concentration and aerogel dosage increase, the plant survival time increases. When the salt concentration is 0.05g / mL, the survival time has reached the longest, which is 5-12 days longer than the control group based on sand. This further illustrates that the atmospheric water collection function of calcium-based aerogel can provide water for plants and prolong their survival time.

[0074] Taking into account the plant height, leaf moisture content, biomass and survival time, calcium aerogel with a salt concentration of 0.05 g / mL was ultimately selected to construct the vegetation layer.

[0075] like Fig.14The adsorption curves of pure PAM-CS matrix and PAM-CS-CaCl2 aerogel at 90% relative humidity. Under the same conditions, the adsorption capacity of PAM-CS-CaCl2 aerogel is as high as 3.76g / g, which is 8.5 times that of PAM-CS. This shows that CaCl2, as the hygroscopic component of hygroscopic aerogel, plays a major role in the atmospheric water collection performance, while the PAM-CS matrix, as the aerogel skeleton loaded with hygroscopic salt, provides channels and carriers for the transmission and storage of liquid water.

[0076] like Fig.15 As shown in the figure, the moisture absorption capacity of calcium-based aerogel-sand increases with the increase of calcium-based aerogel dosage. When exposed to 90% RH and 20℃, the moisture absorption capacity of calcium-based aerogel-sand with a dosage of 2.4% is as high as 0.1 g / g, which is 2 orders of magnitude higher than that of sand. Saturated calcium-based aerogel-sand and pure sand samples were dried at 20% RH and 40℃ to simulate typical dryland weather conditions to evaluate their water holding capacity. Pure sand has almost no water holding capacity, with only 25% of the water content remaining on the first day, while sand doped with PAM-CS-CaCl2 retains 90% of the water, and the remaining water content remains stable at about 10% on the 28th day. The significantly improved moisture collection and water holding capacity provides a promising platform for crop cultivation that does not rely on liquid water resources.

[0077] To verify that the water holding capacity of calcium-based aerogel is not only due to the water retention of PAM-CS matrix, but mainly due to the continuous absorption of liquid water from the atmosphere by calcium-based aerogel to maintain its own moisture, we placed the adsorption-saturated aerogel indoors for release test. During the 18-day release test, the average relative humidity in the room was 63.06% and the average temperature was 20.0℃. Fig.16 b The water stored in the PAM-CS matrix almost completely evaporated on the third day, while the water content in PAM-CS-CaCl2 remained stable at around 15% after 18 days. The volume of PAM-CS aerogels shrank significantly after water loss, while the hygroscopic PAM-CS-CaCl2 calcium-based aerogels maintained a large volume after 18 days ( Fig.16 c). This indicates that the water in the calcium-based aerogel is retained not only because of the water-retaining effect of the matrix, but mainly because of the water-collecting property, which enables it to continuously absorb water from the air to fill the matrix. This further proves the water-holding effect of PAM-CS-CaCl2 due to its water-collecting property.

[0078] Pot test results show that calcium-based aerogel can delay the time it takes for ryegrass to wither and extend the growth time of the plant. Fig.17a After 10 days of stopping water supply, the ryegrass plants in the blank group had already completely withered, while the effect of the PAM-CS matrix without moisture absorption capacity as a water retaining agent in extending the plant growth time was significantly inferior to that of PAM-CS-CaCl2, and its plant vitality was lower than that of the plants treated with PAM-CS-CaCl2.

[0079] Judging from the moisture level of the soil on the surface of the potted plant ( Fig.17 b), the surface soil treated by the CK group and the PAM-CS group showed dry, loose granular sand with a light color due to the evaporation of water and the influence of wind; while the surface of the sand treated by PAM-CS-CaCl2 was moist, the sand became denser, and the color was brown. This is because the hygroscopic calcium-based aerogel PAM-CS-CaCl2 absorbs atmospheric water from the air through the pores of the sand, converts it into liquid water, stores part of it, and uses part of it to supply the water needed for plant growth, while increasing the soil moisture content and prolonging the growth time of plants under drought stress.

[0080] like Fig.17 c. All plants treated with CK group and PAM-CS matrix group died after 8 and 18 days of drought stress, respectively, while the survival rate of PAM-CS-CaCl2 group with water-collecting property was still 100% after 20 days of drought stress. This further proves that PAM-CS-CaCl2 regulates the function of the vegetation layer, which is not only the water-retaining effect of PAM-CS aerogel matrix, but also the water-holding effect of PAM-CS-CaCl2 due to its water-collecting property.

[0081] Fig.18 a shows the moisture absorption performance of sand in an environment of 90%RH and 25℃ under different aerogel content of PAM-CS-CaCl2. The moisture content of sand without aerogel was 0.7% after 36 hours. As the aerogel content increased from 0.4% to 3.2%, the moisture content of sand increased from 4.36% to 21.43%. Fig.18 b shows the PFO model fitting results. The adsorption rate constant of sand without aerogel is 0.00383 min -1 When the aerogel content increases to 3.2%, the adsorption rate constant increases to 0.00531min -1 The above results show that the addition of aerogel increases the moisture content and water vapor adsorption rate of sand.

[0082] Fig.19 a shows the relationship between time and moisture content of silty loess in 90%RH, 25℃ environment under different aerogel content of PAM-CS-CaCl2. The moisture content of silty loess without aerogel was 5.27% after 36h. As the aerogel content increased from 0.4% to 3.2%, the moisture content of silty loess increased from 8.17% to 23.13%. Fig.18 b shows the PFO model fitting results. The adsorption rate constant of sand without aerogel is 0.00422 min -1 When the aerogel content increases to 3.2%, the adsorption rate constant increases to 0.00518 min -1 The above results show that the addition of aerogel increases the moisture content and water vapor adsorption rate of silty loess.

[0083] Fig. 20 a shows the relationship between time and moisture content of loess in 90%RH, 25℃ environment under different aerogel content of PAM-CS-CaCl2. The moisture content of silty loess without aerogel was 18.83% after 36h. As the aerogel content increased from 0.4% to 3.2%, the moisture content of silty loess increased from 21.29% to 31.20%. Fig. 20 b shows the PFO model fitting results. The adsorption rate constant of sand without aerogel is 0.00358 min -1 When the aerogel content increases to 3.2%, the adsorption rate constant increases to 0.00456 min -1 The above results show that the addition of aerogel increases the moisture content and water vapor adsorption rate of yellow clay.

[0084] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A material for constructing a vegetation layer capable of absorbing moisture from the air, characterized in that: include: polymer gel matrix; and a hydrophilic natural polymer loaded on the polymer gel matrix; and deliquescent salts.

2. The material for constructing a vegetation layer capable of absorbing air moisture according to claim 1, characterized in that: The polymer gel matrix comprises at least one of poly(acrylic acid), poly(vinyl pyrrolidone), poly(acrylamide), poly(ethylene oxide), poly(vinyl alcohol), poly(2-hydroxyethyl vinyl ether) and poly(N-isopropylacrylamide).

3. The material for constructing a vegetation layer capable of absorbing air moisture according to claim 1, characterized in that: The hydrophilic natural macromolecule loaded on the polymer gel matrix is ​​selected from one or more of chitosan, starch or sodium alginate.

4. The material for constructing a vegetation layer capable of absorbing air moisture according to claim 1, characterized in that: Deliquescent salts are chlorides or nitrates.

5. The material for constructing a vegetation layer capable of absorbing air moisture according to claim 4, characterized in that: The nitrate is zinc nitrate or calcium nitrate; the chloride is selected from any one of lithium chloride LiCl, calcium chloride CaCl2, magnesium chloride MgCl2, zinc chloride or ferric chloride FeCl3.

6. A method for preparing a material for constructing a vegetation layer capable of absorbing air moisture as claimed in any one of claims 1 to 5, characterized in that: include: forming a polymer gel matrix loaded with hydrophilic natural polymers; Freeze-drying a polymer gel matrix loaded with hydrophilic natural polymers to form a polymer aerogel; and The polymer aerogel is immersed in a solution containing a deliquescent salt, and the polymer aerogel is taken out and dried to obtain the material for constructing a vegetation layer capable of absorbing moisture from the air.

7. The method for preparing a material for constructing a vegetation layer capable of absorbing moisture from the air according to claim 6, characterized in that: The polymer gel matrix for forming a hydrophilic natural macromolecule load comprises: Dissolving a hydrophilic natural polymer in a solvent to form a hydrophilic natural polymer solution; Mixing the monomers of the polymer gel matrix with the hydrophilic natural polymer solution to dissolve the monomers to obtain a monomer mixture; A crosslinking agent and an initiator are added to the monomer mixture, and the mixture is stirred to react to form a polymer gel matrix loaded with hydrophilic natural polymers.

8. The method for preparing a material for constructing a vegetation layer capable of absorbing air moisture according to claim 6, characterized in that: The freeze drying comprises: washing the polymer gel matrix with deionized water and soaking it to swell, then pre-freezing it at -20°C for 12 hours, and then continuing vacuum freeze drying for 48 hours until the sample is dry to form a polymer aerogel; the concentration of the deliquescent salt solution is 0.0125 g / mL-0.05 g / mL.

9. The method for preparing a material for constructing a vegetation layer capable of absorbing air moisture according to claim 7, characterized in that: The solvent is selected from an organic acid solution or water; preferably, the organic acid solution is selected from an acetic acid solution or a propionic acid solution; preferably, the monomer of the polymer gel matrix is ​​selected from acrylamide, N-isopropylacrylamide, acrylic acid, N-vinylpyrrolidone, ethylene oxide, vinyl acetate, 2-hydroxyethyl vinyl ether; preferably, the crosslinking agent is selected from N,N'-methyleneacrylamide MBA; preferably, the initiator is selected from potassium persulfate or ammonium persulfate.

10. A vegetation layer capable of absorbing moisture from the air, characterized in that: It comprises the material and vegetation soil for constructing a vegetation layer capable of absorbing moisture from the air as described in any one of claims 1 to 6; the dosage of the material for constructing a vegetation layer capable of absorbing moisture from the air is 0.3%-2.4%.