Pt-based catalyst taking aluminum oxide as carrier as well as preparation method and application of Pt-based catalyst
By using an alumina-supported Pt-based catalyst and a small particle absorbing medium in the microwave dehydrogenation catalyst, the problems of high microwave heating power and poor matching are solved, and efficient methylcyclohexane dehydrogenation and high-purity hydrogen production are achieved. , has good stability and anti-deactivation properties.
Patent Information
- Application Number
- CN202410677812.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2024-10-22
AI Technical Summary
Existing microwave dehydrogenation catalysts have problems such as high microwave heating power, poor matching between the dehydrogenation catalyst and the absorbing carrier, and poor stability, resulting in low dehydrogenation efficiency and selectivity of methylcyclohexane.
A Pt-based catalyst with alumina as the carrier is used to swing the pH through a sulfuric acid aqueous solution and a sodium metaaluminate aqueous solution, ultrasonic impregnation of Pt and K loads, combined with small particle absorbing media, to form a bed filler for microwave-assisted methylcyclohexane Alkane dehydrogenation reaction.
It significantly improves the dehydrogenation conversion rate and hydrogen selectivity of methylcyclohexane, enhances the anti-deactivation ability of the catalyst, and improves the heating efficiency and stability of the catalytic reaction.
Smart Images

Figure BDA0004864722200000121 
Figure BDA0004864722200000131 
Figure HDA0004864722210000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of chemical hydrogen storage, and in particular relates to a Pt-based catalyst using aluminum oxide as a carrier, and a preparation method and application thereof. Background Art
[0002] The increasing depletion of fossil energy and the environmental problems caused by its development and utilization have forced people to develop green and environmentally friendly renewable energy. Hydrogen energy, as an ideal fuel, has received increasing attention. However, gaseous hydrogen is large in volume, difficult to store and transport, prone to leakage and has the risk of explosion, so it is necessary to develop efficient hydrogen storage technology. The methylcyclohexane-toluene system has the potential to store and transport hydrogen over long distances due to its low cost, relatively low toxicity and good safety.
[0003] The dehydrogenation reaction of methylcyclohexane (MCH) is endothermic. Conventional thermal reactors usually transfer heat from the walls and cavity of the tube furnace to the catalyst through conduction and convection mechanisms, but this will lead to energy loss. In contrast, the use of microwave energy to heat the reactor can form microplasma in a short time, improve the activity of the catalyst, and thus improve energy utilization efficiency, which has more advantages (Science Advances, 2023, 9, eadi8219). At present, research on the dehydrogenation of liquid organic hydrides in microwave reactors is relatively limited. Combining a microwave reactor that reduces the dead zone of the catalyst temperature with a Pt-based catalyst is expected to further improve the dehydrogenation efficiency of MCH.
[0004] The patent document with the publication number CN103951540A discloses a microwave heating application method of an integral nano-carbon composite catalyst, in which a Pd-impregnated carbon-based absorbing medium is used in a reactor to carry out dehydrogenation reaction of organic hydrogen storage liquids such as decahydronaphthalene and perhydrofluorene. After heating at 1000W microwave for 300min, the conversion rates of decahydronaphthalene and perhydrofluorene were only 13.8% and 2.3%, respectively.
[0005] Patent document with publication number CN116060072A discloses a microwave dehydrogenation catalyst and its preparation method. By adding Pt-absorbing medium silicon carbide ceramic powder to 3D print Pt-SiC catalyst, microwave heating at 500°C in ethane dehydrogenation reaction achieved 73% ethane conversion rate and 85% ethylene selectivity. However, the printing temperature of 1450°C seriously affected the service life of 0.3wt% Pt-based catalyst.
[0006] In summary, microwave dehydrogenation catalysts currently have the following main problems: high microwave heating power, poor matching between the dehydrogenation catalyst and the microwave absorbing carrier, poor stability, etc. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the present invention provides a Pt-based catalyst using aluminum oxide as a carrier, a preparation method and an application thereof. The preparation method is simple to operate and takes a short heating time. The prepared Pt-based catalyst has high methylcyclohexane conversion rate, hydrogen selectivity and anti-deactivation ability when used for microwave-assisted methylcyclohexane (MCH) catalytic dehydrogenation.
[0008] A method for preparing a Pt-based catalyst using aluminum oxide as a carrier comprises the following steps:
[0009] (1) pH swing is performed three times using a sulfuric acid aqueous solution and a sodium aluminate aqueous solution, and the suspension after the swing is filtered, washed, dried and calcined in sequence to obtain a γ-Al2O3 carrier;
[0010] (2) using chloroplatinic acid aqueous solution as an impregnation solution, loading Pt onto the γ-Al2O3 carrier under ultrasonic action, and then drying and calcining to obtain the Pt / Al2O3 catalyst;
[0011] (3) Using KNO3 aqueous solution as the impregnation solution, K is loaded onto the Pt / Al2O3 catalyst under the action of ultrasound, and then dried to obtain the Pt-based catalyst with alumina as the carrier.
[0012] In the above step (1):
[0013] Preferably, during the pH swing, the pH in the acidic region is 2 to 5, and the pH in the alkaline region is 7 to 11. More preferably, during the pH swing, the pH in the acidic region is 2 to 3, and the pH in the alkaline region is 9 to 10. Even more preferably, during the pH swing, the pH in the acidic region is 2, and the pH in the alkaline region is 10.
[0014] Preferably, the drying temperature is 70 to 90° C., and the drying time is 2 to 4 hours. More preferably, the drying temperature is 80° C., and the drying time is 3 hours.
[0015] Preferably, the calcination temperature is 400-800°C and the calcination time is 3-5 hours. More preferably, the calcination temperature is 400-600°C and the calcination time is 3-4 hours. More preferably, the calcination temperature is 500°C and the calcination time is 3 hours.
[0016] In the above step (2):
[0017] Preferably, the drying temperature is 70-90° C., and the drying time is 2-4 h; more preferably, the drying temperature is 80° C., and the drying time is 3 h.
[0018] Preferably, the calcination temperature is 300-500°C and the calcination time is 1-5 hours. More preferably, the calcination temperature is 350-450°C and the calcination time is 2-4 hours. More preferably, the calcination temperature is 400°C and the calcination time is 3 hours.
[0019] Preferably, the calcination atmosphere is one of hydrogen, air and nitrogen, and more preferably hydrogen.
[0020] Preferably, Pt is loaded by an equal volume impregnation method, and the ultrasonic time during the equal volume impregnation is 5 to 30 minutes, more preferably 8 to 15 minutes, and even more preferably 10 minutes.
[0021] Preferably, the Pt loading in the Pt / Al2O3 catalyst is 0.5 to 5 wt %, more preferably 0.5 to 2 wt %, and even more preferably 0.6 wt %.
[0022] In the above step (3):
[0023] Preferably, in the Pt-based catalyst with alumina as the carrier, the K loading is 0.01 to 2 wt %, more preferably 0.05 to 1 wt %, and even more preferably 0.1 to 0.5 wt %.
[0024] Preferably, K is loaded by equal volume impregnation method, and the ultrasonic time during equal volume impregnation is 5 to 30 minutes, more preferably 8 to 15 minutes, and even more preferably 10 minutes.
[0025] Preferably, the drying temperature is 70-90° C., and the drying time is 2-4 h; more preferably, the drying temperature is 80° C., and the drying time is 3 h.
[0026] As a specific preference, a method for preparing a Pt-based catalyst using aluminum oxide as a carrier comprises the following steps:
[0027] The aqueous sulfuric acid solution is added to deionized water and mixed thoroughly to obtain an acidic solution; the aqueous sodium aluminate solution is added thereto and mixed evenly to complete the first pH swing; the catalytic process undergoes three pH swings, and the suspension after the swing is filtered and washed to obtain a γ-Al2O3 precursor; the γ-Al2O3 precursor is dried and calcined to obtain a γ-Al2O3 carrier;
[0028] Under the action of ultrasound, the chloroplatinic acid impregnation solution (chloroplatinic acid aqueous solution) is loaded onto the γ-Al2O3 carrier by an equal volume impregnation method to obtain a Pt / Al2O3 precursor; the Pt / Al2O3 precursor is dried and calcined to obtain a Pt / Al2O3 catalyst;
[0029] KNO3 is dissolved in deionized water to prepare an impregnation solution, and K is loaded onto a Pt / Al2O3 catalyst under the action of ultrasound using an equal volume impregnation method to obtain a PtK / Al2O3 catalyst precursor; the PtK / Al2O3 precursor is dried to obtain a PtK / Al2O3 catalyst.
[0030] A Pt-based catalyst with aluminum oxide as a carrier is prepared by any of the above-mentioned methods for preparing a Pt-based catalyst with aluminum oxide as a carrier.
[0031] A method for microwave-assisted dehydrogenation of methylcyclohexane comprises the following steps:
[0032] (1) The above-mentioned Pt-based catalyst with alumina as a carrier is mixed with a microwave absorbing medium and then filled into a microwave fixed bed reaction tube as a bed filler;
[0033] (2) After being vaporized, methylcyclohexane is introduced into the microwave fixed bed reaction tube to undergo a high temperature catalytic reaction under microwave-assisted heating and induction conditions and accompanied by hydrogen. The reaction product and the raw material are condensed and separated to obtain a liquid product and a gas product.
[0034] Preferably, the absorbing medium (Y) is one or more of silicon carbide, activated carbon, and metal alloy.
[0035] As a further preference, the absorbing medium is silicon carbide or activated carbon.
[0036] The particle size of silicon carbide is 10 to 200 mesh, preferably 16 to 100 mesh, and more preferably 80 to 100 mesh.
[0037] The particle size of the activated carbon is 10 to 200 mesh, preferably 16 to 100 mesh, and more preferably 80 to 100 mesh.
[0038] As further preferred, the absorbing medium is silicon carbide.
[0039] Preferably, the mass ratio of the Pt-based catalyst with alumina as a carrier to the absorbing medium is (1-5):1, and more preferably (1-3):1.
[0040] As a specific preference, in the bed filler, the mass of the Pt-based catalyst supported by alumina is 200 mg.
[0041] Preferably, methylcyclohexane is pumped into the gasifier via a liquid pump for gasification, and the liquid pump pumping flow rate is 0.01 to 0.5 mL / min, more preferably 0.05 to 0.2 mL / min, and even more preferably 0.05 to 0.1 mL / min.
[0042] The gasification temperature of the gasifier is 100 to 200°C, preferably 150°C.
[0043] Preferably, the microwave-assisted heating and induction power is 100 to 1200 W, more preferably 300 to 1200 W, and even more preferably 300 to 500 W.
[0044] Preferably, the accompanying flow rate of hydrogen is 0.1 to 20 mL / min, more preferably 5 to 10 mL / min.
[0045] Preferably, the reaction temperature of the catalytic reaction is 300 to 400°C, more preferably 350°C.
[0046] Preferably, the reaction product and the raw material are condensed and separated in a gas-liquid separation tank, wherein the condensation temperature is 2-6° C. More preferably, the condensation temperature is 4° C.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The method for preparing a Pt-based catalyst with alumina as a carrier of the present invention comprises the following steps: preparing γ-Al2O3 by a pH swing one-step method, and then preparing a PtK / Al2O3 catalyst (Pt-based catalyst with alumina as a carrier) by an equal volume impregnation method; mixing the prepared Pt-based catalyst with alumina as a carrier with an absorbing medium to obtain a bed filler PtK / Al2O3&Y, which can effectively absorb microwaves, significantly enhance heat transfer, and has the characteristics of fast heating speed, selective heating and high heating efficiency; the bed filler is used in a microwave-assisted catalytic dehydrogenation process of methylcyclohexane, and has a high conversion rate and stability, and the product has high hydrogen purity and low methane selectivity. The coupling of the absorbing medium and the Pt-based catalyst improves the dehydrogenation conversion rate of methylcyclohexane. In the catalytic dehydrogenation process of methylcyclohexane, the stability of the catalytic dehydrogenation of methylcyclohexane can be increased under the conditions of small-particle absorbing medium and low-rate methylcyclohexane feed. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 is the X-ray diffraction (XRD) pattern of the Pt-based catalysts prepared in Examples 1 to 7;
[0050] Figure 2 The particle size distribution and TEM images of the Pt-based catalysts prepared in Examples 3 to 7;
[0051] Figure 3 This is a graph showing the results of the long-term performance evaluation of the bed filler prepared in Example 7 for the dehydrogenation reaction of methylcyclohexane. DETAILED DESCRIPTION
[0052] In order to better understand the present invention, the present invention is described in detail below in conjunction with specific embodiments. In order to elaborate on the present invention, the following examples illustrate many process details, which are not intended to cause improper limitations on the present invention.
[0053] The purity of methylcyclohexane (MCH) used in the following examples is greater than 99%.
[0054] [Example 1]
[0055] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0056] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0057] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 1 wt% K-loaded Pt-based catalyst (Pt 0.6 K 1.0 / Al2O3 catalyst).
[0058] 200 mg of Pt-based catalyst powder and 16-mesh absorbing medium silicon carbide were physically mixed in a ratio of 3:1, and the two were fully mixed to form the microwave fixed bed filler Pt 0.6 K 1.0 / Al2O3&SiC-16(3:1).
[0059] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and the raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 300W, the accompanying flow rate of hydrogen is 10mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.1mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0060] [Example 2]
[0061] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0062] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0063] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 0.5 wt% K-loaded Pt-based catalyst (Pt 0.6 K 0.5 / Al2O3 catalyst).
[0064] 200 mg of Pt-based catalyst powder and 16-mesh absorbing medium silicon carbide were physically mixed in a ratio of 3:1, and the two were fully mixed to form the microwave fixed bed filler Pt 0.6 K 0.5 / Al2O3&SiC-16(3:1).
[0065] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and the raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 300W, the accompanying flow rate of hydrogen is 10mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.1mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0066] [Example 3]
[0067] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0068] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0069] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 0.1 wt% K-loaded Pt-based catalyst (Pt 0.6 K 0.1 / Al2O3 catalyst).
[0070] 200 mg of Pt-based catalyst powder and 16-mesh absorbing medium silicon carbide were physically mixed in a ratio of 3:1, and the two were fully mixed to form the microwave fixed bed filler Pt 0.6 K 0.1 / Al2O3&SiC-16(3:1).
[0071] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and the raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 300W, the accompanying flow rate of hydrogen is 10mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.1mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0072] [Example 4]
[0073] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0074] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0075] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 0.1 wt% K-loaded Pt-based catalyst (Pt 0.6 K 0.1 / Al2O3 catalyst).
[0076] 200 mg of Pt-based catalyst powder and 100-mesh absorbing medium silicon carbide were physically mixed in a ratio of 1:1, and the two were fully mixed to form the microwave fixed bed filler Pt0.6 K 0.1 / Al2O3&SiC-100(1:1).
[0077] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and the raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 1200W, the accompanying flow rate of hydrogen is 10mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.2mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0078] [Example 5]
[0079] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0080] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0081] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 0.1 wt% K-loaded Pt-based catalyst (Pt 0.6 K 0.1 / Al2O3 catalyst).
[0082] 200 mg of Pt-based catalyst powder and 16-mesh activated carbon were physically mixed at a mass ratio of 3:1 between the Pt-based catalyst and the absorbing medium. The two were fully mixed to form the microwave fixed bed filler Pt 0.6 K 0.1 / Al2O3&C-16(3:1).
[0083] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 300W, the accompanying flow rate of hydrogen is 5mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.05mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0084] [Example 6]
[0085] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0086] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0087] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 0.1 wt% K-loaded Pt-based catalyst (Pt 0.6 K 0.1 / Al2O3 catalyst).
[0088] 200 mg of Pt-based catalyst powder and 100-mesh activated carbon were physically mixed in a ratio of 1:1 between the mass ratio of Pt-based catalyst and the absorbing medium. The two were fully mixed to form the microwave fixed bed filler Pt 0.6 K 0.1 / Al2O3&C-100(1:1).
[0089] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and the raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 1200W, the accompanying flow rate of hydrogen is 10mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.1mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0090] [Example 7]
[0091] Add an appropriate amount of 15wt% sulfuric acid aqueous solution to 1L deionized water, mix evenly under the action of a rotating stirring paddle to obtain an acidic solution with a pH of 2. Slowly add 2mol / L sodium aluminate aqueous solution to the acidic solution until the pH reaches 10 and stop adding, completing the first pH swing. During this period, sodium aluminate initially hydrolyzes under acidic conditions and then tends to alkaline hydrolysis. Then repeat the above operation and perform pH swings twice to obtain a suspension of pseudo-boehmite precursor. Filter the suspension in a suction flask, then wash with 5L deionized water, and finally dry at 80°C for 3h and place it in a muffle furnace and roast it at 500°C for 3h to obtain a γ-Al2O3 carrier.
[0092] Chloroplatinic acid was prepared into an aqueous solution (each mL of aqueous solution contained 39.2 μg of Pt), and the chloroplatinic acid aqueous solution was impregnated on the γ-Al2O3 support by an equal volume impregnation method under the action of ultrasound (10 min). The impregnated slurry was then dried at 80°C for 3 h and transferred to a tubular furnace reactor and calcined at 400°C for 3 h by passing 10 mL / min of hydrogen to obtain a 0.6 wt% Pt-loaded Pt-based catalyst (Pt 0.6 / Al2O3 catalyst).
[0093] Under the action of ultrasound (10 min), KNO3 aqueous solution was impregnated on Pt by equal volume impregnation method. 0.6 / Al2O3 catalyst, and then the impregnation slurry was placed at 80 ° C for 3 h to obtain a 0.1 wt% K-loaded Pt-based catalyst (Pt 0.6 K0.1 / Al2O3 catalyst).
[0094] 200 mg of Pt-based catalyst powder and 100-mesh absorbing medium silicon carbide were physically mixed in a ratio of 3:1. The two were fully mixed to form the microwave fixed bed filler Pt 0.6 K 0.1 / Al2O3&SiC-100(3:1).
[0095] After methylcyclohexane is pumped into a gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction and hydrogen accompanying conditions, and the reaction product and raw material are condensed and separated into liquid phase products and gas phase products through a gas-liquid separation tank. Among them, the microwave power for dehydrogenation of methylcyclohexane is 300W, the accompanying flow rate of hydrogen is 5mL / min, the flow rate of methylcyclohexane pumped into the liquid pump is 0.05mL / min, the gasification temperature of the gasifier is 150°C, the microwave fixed bed reaction temperature (catalytic reaction temperature) is 350°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0096] Product Characterization:
[0097] The XRD patterns of the Pt-based catalysts prepared in Examples 1 to 7 are as follows: Figure 1 As shown by Figure 1 It can be seen that the Pt-based catalysts prepared in Examples 1 to 7 all show the characteristic peak of γ-Al2O3, and as the amount of K added increases, the crystallinity of the Pt-based catalyst decreases.
[0098] The Pt prepared in Examples 3 to 7 0.6 K 0.1 The particle size distribution (TEM) of the / Al2O3 catalyst is shown in Figure 2 As shown by Figure 2 It can be seen that the Pt particles of the catalyst are evenly dispersed and have an average particle size of 1.3 nm.
[0099] Performance Test:
[0100] The products (gas phase products and liquid phase products) obtained in Examples 1 to 7 were analyzed by gas chromatography, wherein the results of the catalytic dehydrogenation reaction for 1 hour are shown in Table 1; meanwhile, the product analysis results of the methylcyclohexane dehydrogenation reaction after 24 hours are shown in Table 2.
[0101] Table 1 Product analysis results of methylcyclohexane dehydrogenation catalysis for 1 h
[0102]
[0103] It can be seen from Table 1 that the microwave fixed bed fillers prepared in Examples 1 to 7, especially the microwave fixed bed fillers prepared in Example 7, have a high microwave matching degree between the Pt-based catalyst powder and the 100-mesh SiC. When the catalyst with a Pt loading of 0.6wt% and a K loading of 0.1wt% is used to catalyze the dehydrogenation reaction of methylcyclohexane, methylcyclohexane has a high conversion rate, and the selectivity for methane and the purity of hydrogen in the product (ultra-low methane concentration) are both excellent.
[0104] Table 2 Product analysis results of methylcyclohexane dehydrogenation catalysis for 24h
[0105]
[0106] It can be seen from Table 2 that the Pt-based catalysts prepared in Examples 1 to 7 above still have excellent toluene selectivity and hydrogen purity in the catalytic dehydrogenation reaction of methylcyclohexane after 24 hours of catalytic reaction; only the conversion rate of methylcyclohexane decreases, and have excellent anti-deactivation ability.
[0107] The Pt prepared in Example 7 0.6 K 0.1 / Al2O3&SiC-100 (3:1) bed packing was used for 400h long-term catalytic performance evaluation:
[0108] After methylcyclohexane is pumped into the gasifier through a liquid pump for gasification, it is passed into a microwave fixed bed reaction tube (installed with the above-prepared bed filler), and a high-temperature catalytic reaction is carried out under microwave-assisted heating and induction, accompanied by hydrogen. The reaction products and raw materials are condensed and separated into liquid products and gas products through a gas-liquid separation tank. Among them, the evaluation conditions are: the catalytic reaction temperature is 350°C, the reaction pressure is 0.1MPa, the methylcyclohexane liquid flow rate is 0.05mL / min, 0.1mL / min of hydrogen is carried, the gasification temperature of the gasifier is 150°C, and the condensation temperature of the gas-liquid separation tank is 4°C.
[0109] The products (gas phase products and liquid phase products) obtained from the above test were analyzed by gas chromatography, and the results are as follows: Figure 3 As shown. Figure 3 It can be seen that in the long-term evaluation of 400 h, the microwave-assisted methylcyclohexane dehydrogenation catalyst (Pt 0.6 K 0.1 / Al2O3) has excellent performance, the content of methane by-products continues to remain at a low level, the methylcyclohexane conversion rate drops from 99.9% to 98.5%, and the toluene selectivity continues to remain at 99.9%, with excellent stability.
[0110] It can be seen from the performance test results of the above embodiments that the microwave fixed bed filler provided by the present invention has a higher methylcyclohexane conversion rate and better stability when used for methylcyclohexane dehydrogenation reaction.
[0111] The above description is only a preferred embodiment of the present invention. It should be pointed out that for those skilled in the art, several improvements and modifications made within the scope of the principle of the present invention should also be regarded as the protection scope of the present invention.
Claims
1. A method for preparing a Pt-based catalyst using aluminum oxide as a carrier, characterized in that: The following steps are involved: (1) subjecting a sulfuric acid aqueous solution and a sodium aluminate aqueous solution to pH swing three times, and filtering, washing, drying and calcining the suspension after the swing in sequence to obtain a γ-Al2O3 carrier; (2) using chloroplatinic acid aqueous solution as an impregnation solution, loading Pt onto the γ-Al2O3 carrier under ultrasonic action, and then drying and calcining to obtain the Pt / Al2O3 catalyst; (3) Using KNO3 aqueous solution as the impregnation solution, K is loaded onto the Pt / Al2O3 catalyst under the action of ultrasound, and then dried to obtain the Pt-based catalyst with alumina as the carrier.
2. The method for preparing a Pt-based catalyst with aluminum oxide as a carrier according to claim 1, characterized in that: During the pH swing, the pH in the acidic region is 2 to 5, and the pH in the alkaline region is 7 to 11.
3. The method for preparing a Pt-based catalyst with aluminum oxide as a carrier according to claim 1, characterized in that: In step (1), the calcination temperature is 400-800° C. and the calcination time is 3-5 hours.
4. The method for preparing a Pt-based catalyst with alumina as a carrier according to claim 1, characterized in that: In step (2), the calcination temperature is 300 to 500° C. and the calcination time is 1 to 5 hours; The calcination atmosphere is one of hydrogen, air and nitrogen.
5. The method for preparing a Pt-based catalyst with alumina as a carrier according to claim 1, characterized in that: In the Pt / Al2O3 catalyst, the loading amount of Pt is 0.5 to 5 wt%.
6. The method for preparing a Pt-based catalyst with alumina as a carrier according to claim 1, characterized in that: In the Pt-based catalyst with alumina as the carrier, the loading amount of K is 0.01 to 2 wt%.
7. The method for preparing a Pt-based catalyst with alumina as a carrier according to claim 1, characterized in that: In steps (2) and (3), Pt and K are loaded respectively by equal volume impregnation method, and the ultrasonic time during equal volume impregnation is 5 to 30 minutes.
8. A Pt-based catalyst with aluminum oxide as a carrier, characterized in that: The catalyst is prepared by the method for preparing a Pt-based catalyst using aluminum oxide as a carrier according to any one of claims 1 to 7.
9. A method for microwave-assisted dehydrogenation of methylcyclohexane, characterized in that: The following steps are involved: (1) The Pt-based catalyst with alumina as a carrier as claimed in claim 8 is mixed with a microwave absorbing medium and then filled into a microwave fixed bed reaction tube as a bed filler; (2) After being vaporized, methylcyclohexane is introduced into the microwave fixed bed reaction tube to undergo a high temperature catalytic reaction under microwave-assisted heating and induction conditions and accompanied by hydrogen. The reaction product and the raw material are condensed and separated to obtain a liquid product and a gas product.
10. The method for microwave-assisted dehydrogenation of methylcyclohexane according to claim 9, characterized in that: The mass ratio of the Pt-based catalyst with alumina as the carrier to the absorbing medium is (1-5):1; The absorbing medium is one or more of silicon carbide, activated carbon, and metal alloy.
Citation Information
Patent Citations
Method for adsorbing carbon monoxide
JP1987108724A
Hydrogen gas formation apparatus
JP2004002090A
Platinum-loaded alumina catalyst, method of producing same, and method of dehydrogenating hydrogenated aromatic using the catalyst
US20230338927A1
Cited By
Pt cluster catalyst, preparation method and application
CN120037905A
A Pt cluster catalyst, preparation method and application
CN120037905B
Adsorption coupling catalyst, preparation method thereof and application of adsorption coupling catalyst in catalytic adsorption of methyl mercaptan and carbon dioxide
CN120393990A