Fe-doped sargassum horneri biochar as well as preparation and application thereof
By doping copper algae biochar with iron ions, Fe-doped copper algae biochar was prepared and PDS was activated, which solved the problem of low efficiency of iron ion activation of PDS and achieved efficient removal of tetracycline.
Patent Information
- Application Number
- CN202410705344.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-22
AI Technical Summary
When the existing technology activates persulfate (PDS), the electron utilization rate of iron ions (Fe3+) is low, the recyclability is poor, and secondary pollution is generated, making it difficult to efficiently remove tetracycline (TC) pollution.
Iron trichloride hexahydrate (FeCl3·6H2O) was used as the iron source, and Fe-doped copper algae biochar was prepared by impregnation-calcination method, which was used to activate PDS, thereby improving its efficiency in removing tetracycline.
It significantly improves the oxidation activity of PDS, achieves efficient removal of tetracycline, reduces the problems of poor electron utilization and recyclability, and avoids secondary pollution.
Smart Images

Figure SMS_1 
Figure HDA0004872313490000011 
Figure HDA0004872313490000012
Abstract
Description
Technical Field
[0001] The present invention relates to the field of medical technology, and in particular to Fe-doped copper algae biochar, preparation thereof and application thereof. Background Art
[0002] Tetracycline (TC) is a typical antibiotic widely used in clinical medicine and animal husbandry. However, TC is easily discharged into the water environment after biological digestion and metabolism, posing a major threat to the environment. It is particularly important to study efficient and economical TC removal technology. Among them, AOPs have been widely used in the degradation of organic pollutants, especially PDS-based advanced oxidation technology, which can produce active oxygen groups with strong oxidation potential, mainly SO4 ·- , its redox potential is as high as 2.5-3.1V. In addition, PDS has the advantages of high selectivity and long duration, and has received increasing attention in the removal of organic pollutants. However, PDS itself has limited oxidative activity against organic pollutants because it is relatively stable under normal conditions. Common applications include UV, ultrasound, transition metals and carbon-based materials to activate PDS to produce more active oxygen. At present, the transition metals commonly used to activate PDS are cobalt, nickel, copper, silver, manganese, iron, etc. Among them, iron ions (Fe 3+ ) has become the preferred agent for activating PDS due to its low toxicity, rich valence states and excellent activation performance. 3+ In the process of activating PDS, there are still disadvantages such as low electron utilization, poor recyclability and secondary pollution. Therefore, it is necessary to explore methods to prevent ion oxidation and release.
[0003] Sargassum horneri is a type of brown algae that grows fast and does not occupy arable land. Considering the rich pore structure of Sargassum horneri and the availability of its own nitrogen doping, converting Sargassum horneri into biochar may be an effective method to prepare Sargassum horneri biochar-based catalysts with high specific surface area, multifunctional groups and more PDS activation active centers. At present, there is a lack of research on the use of Sargassum horneri as a biochar precursor to prepare composite materials. Summary of the invention
[0004] The present invention selects copper algae biomass as biochar precursor, adopts ferric chloride hexahydrate (FeCl3·6H2O) as iron source, prepares Fe-doped copper algae biochar composite material by impregnation-calcination method, and uses it to activate persulfate (PDS), providing a new method for removing tetracycline (TC) using copper algae biochar-derived catalyst.
[0005] In one aspect, the present invention provides a method for preparing Fe-doped copper algae biochar, which comprises the following steps:
[0006] 1) Pretreatment of copper algae: soak and rinse the copper algae with deionized water until there is no obvious impurity, dry and crush, sieve, and obtain copper algae powder for later use;
[0007] 2) Preparation of copper algae biochar: copper algae powder was placed in a square corundum crucible and calcined in a tube furnace. After calcination, it was cooled to room temperature, rinsed with deionized water until neutral, and dried to obtain copper algae biochar BC;
[0008] 3) Preparation of Fe-doped copper algae biochar
[0009] The copper algae biochar BC in step 2) is weighed, immersed in a FeCl3·6H2O solution, and stirred to allow the copper algae biochar BC to fully absorb the iron salt. Then, the BC absorbing different concentrations of iron salts is placed in a drying oven to dry to obtain a precursor of the mixed material; then, the precursor is transferred to a square corundum crucible, placed in a tubular furnace, and calcined to obtain Fe-doped copper algae biochar Fe@BC.
[0010] Preferably, the sieving in step 1) is 100 mesh.
[0011] Preferably, the calcination procedure in step 2) is: introducing 99.999% high-purity N2 at a flow rate of 100 mL / min, and exhausting the air in the furnace for 30 minutes; heating from room temperature to 200°C at a heating rate of 10°C / min, maintaining for 30 minutes, and then heating from 200°C to 700°C at the same heating rate, and maintaining for 120 minutes;
[0012] Preferably, the cooling procedure after calcination in step 2) is: reducing the temperature to 300°C at a rate of 10°C / min, turning off the tube furnace and N2, and cooling naturally to room temperature.
[0013] Preferably, the concentration of the FeCl3·6H2O solution in step 3) is 0.03 mol / L-0.3 mol / L.
[0014] Preferably, in step 3), the weight-to-volume ratio of copper algae biochar BC to FeCl3·6H2O solution is 1 g:100 ml.
[0015] Preferably, the calcination procedure in step 3) is as follows: use N2 with a flow rate of 100 mL / min to purge the residual air in the furnace, then set the heating rate to 5°C / min, raise the carbonization temperature to 900°C, carbonize at a constant temperature for 2 hours, reduce the temperature to 300°C at a cooling rate of 5°C / min, then turn off the tubular furnace and wait for the sample to cool to room temperature.
[0016] On the other hand, the present invention provides Fe-doped copper algae biochar prepared by the above method.
[0017] On the other hand, the present invention provides the use of the above-mentioned Fe-doped copper algae biochar in degrading tetracycline (TC).
[0018] Furthermore, the conditions for degrading tetracycline are as follows: the initial pH of the tetracycline (TC) solution is 4.6, the initial temperature is 45°C, the dosage of Fe-doped copper algae biochar Fe@BC is 0.04 g / L, the initial mass concentration of tetracycline (TC) is 20 mg / L, and the concentration of persulfate (PDS) is 1 mmol / L.
[0019] Furthermore, the persulfate (PDS) is preferably potassium persulfate. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 SEM images of different samples (a: BC; b: Fe@BC; c: 3Fe@BC).
[0021] Figure 2 EDS-mapping spectra and element contents of different samples (a: BC; b: Fe@BC; c: 3Fe@BC).
[0022] Figure 3 XRD patterns of different samples.
[0023] Figure 4 TEM and HRTEM images of different Fe loading amounts (a: Fe@BC; b: 3Fe@BC; c: 3Fe@BC).
[0024] Figure 5 N2 adsorption-desorption isotherms and pore size distribution diagrams of different samples (a: N2 adsorption-desorption isotherms; b: pore size distribution diagram)
[0025] Figure 6 FTIR spectra of different samples.
[0026] Figure 7 XPS spectra: a is the full spectrum of different samples; b is the Fe 2p spectrum of Fe@BC.
[0027] Figure 8 Raman spectra of different samples.
[0028] Fig. 9 Effects of different systems on TC degradation: (a) degradation curve, (b) kinetic curve and (c) degradation rate constant.
[0029] Fig.10 Effect of Fe@BC dosage on TC degradation in Fe@BC / PDS system: (a) degradation curve, (b) kinetic curve and (c) degradation rate constant.
[0030] Fig.11 Effect of PDS concentration on TC degradation in Fe@BC / PDS system: (a) degradation curve, (b) kinetic curve and (c) degradation rate constant.
[0031] Fig.12 The effect of initial TC mass concentration on TC degradation by Fe@BC / PDS system.
[0032] Fig.13 The effect of temperature on the degradation of TC by Fe@BC / PDS system.
[0033] Fig.14 The effect of different inorganic anions on the degradation of TC by Fe@BC / PDS system. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below with reference to the accompanying drawings.
[0035] PDS: persulfate. The PDS used in the embodiment of the present invention is potassium persulfate;
[0036] TC: tetracycline;
[0037] Fe@BC: Fe-doped copper algae biochar;
[0038] Copper algae were purchased from Wuzhoufeng Agricultural Technology Co., Ltd.
[0039] Example 1 Preparation of copper algae biochar
[0040] Pretreatment of copper algae: Soak and rinse the purchased copper algae with deionized water until there are no obvious impurities, and dry the washed copper algae in an electric hot air drying oven at 105°C to constant weight. Crush the dried copper algae and sieve through a 100-mesh sieve to obtain copper algae powder for later use.
[0041] Preparation of copper algae biochar: Put the copper algae powder into a square corundum crucible, place it in a tube furnace, and pass 99.999% high-purity N2 at a flow rate of 100mL / min. Ventilate for 30 minutes to exhaust the air in the furnace. Raise the temperature from room temperature to 200℃ at a heating rate of 10℃ / min, hold for 30 minutes, and then increase the temperature from 200℃ to 700℃ at the same heating rate, and hold for 120 minutes. After calcination, reduce the temperature to 300℃ at a rate of 10℃ / min, turn off the tube furnace and N2, and cool naturally to room temperature. Take out the cooled sample and rinse it with deionized water until it is neutral. Place the sample in an electric heated blast drying oven at 60℃ and dry it for 12 hours to obtain a sample, marked as BC.
[0042] Example 2 Preparation of Fe-doped copper algae biochar
[0043] Fe-doped copper algae biochar was synthesized by impregnation-calcination method. First, 1g of BC was weighed and soaked in 100ml FeCl3·6H2O solution with concentration of 0.03mol / L and 0.3mol / L respectively and stirred for 24h to make BC and iron salt fully absorbed. Then, BC absorbing different concentrations of iron salt was placed in a vacuum freeze drying oven for 24h to obtain the precursor of the mixed material. Then, the precursor was transferred to a square corundum crucible and placed in a tube furnace. To ensure an inert atmosphere in the furnace, the residual air in the furnace was purged with N2 at a flow rate of 100mL / min. Then, the heating rate was set to 5℃ / min, the carbonization temperature was raised to 900℃, and the carbonization was carried out at a constant temperature for 2h. The temperature was reduced to 300℃ at a cooling rate of 5℃ / min, and the tube furnace was closed. After the sample cooled to room temperature, it was taken out and packaged in a sample bag. The Fe-doped copper algae biochars were named Fe@BC (corresponding to 0.03 mol / L FeCl3·6H2O) and 3Fe@BC (corresponding to 0.3 mol / LFeCl3·6H2O).
[0044] Example 3 Characterization of Fe-doped copper algae biochar
[0045] The micromorphology, crystal structure, functional groups, and surface element composition of BC, Fe@BC, and 3Fe@BC samples were characterized. The microstructure and surface morphology of the samples were observed by scanning electron microscopy (SEM), and EDS-mapping was performed on BC, Fe@BC, and 3Fe@BC samples to observe the uniformity of the distribution of C, N, O, Si, Al, and Fe elements on the sample surface; the microstructure of the samples was analyzed by high-resolution transmission electron microscopy (HRTEM), and the exposed crystal faces of the samples were analyzed based on the lattice fringe spacing; the specific surface area and pore size distribution of the samples were determined by a specific surface area analyzer (BET), and the specific specific surface area, pore volume, and pore size of the samples were calculated by the BJH method; the chemical functional groups on the sample surface were identified by Fourier transform infrared spectroscopy (FTIR), and the samples were mixed with potassium bromide by potassium bromide tablet method, with a mass ratio of sample to potassium bromide of 200:1, and the scanning range was 4000-400cm -1 ; The physical composition and crystal structure of the samples were tested on an X-ray diffractometer (XRD), using Cu target Ka rays, scanning at a speed of 5° / min, and an angle range of 5° to 90°; the defects and degree of graphitization of the samples were characterized by Raman spectroscopy, with an excitation wavelength of 532nm; the surface element composition, element valence state and element binding energy of the samples were analyzed by X-ray photoelectron spectroscopy (XPS), and the raw data were peak fitted using Avantage software, and energy spectrum correction was performed using C1s (284.8eV).
[0046] Figure 1SEM images of BC, Fe@BC and 3Fe@BC. Figure 1 (a) It can be seen that the surface of BC presents an uneven gully-like structure and contains a large number of fragments, which will become the key positions for loading iron in the later stage. Figure 1 (b) shows the SEM image of Fe@BC. With the introduction of Fe, the originally irregular folds become rough and a large number of rod-shaped crystals appear. This may be due to the inorganic salts contained in the copper algae itself. Figure 1 (c) is the SEM image of 3Fe@BC. With the increase of Fe element, more rod-shaped crystals appear on the surface of the material, which may be due to the change of its structure and morphology caused by iron doping.
[0047] The element distribution of BC, Fe@BC and 3Fe@BC was analyzed by X-ray energy spectrum scanning (EDS-Mapping). The results are shown in Figure 2 ,exist Figure 2 It can be seen that Fe is evenly attached to the sample surface, which further shows that Fe is successfully loaded on BC, and as the Fe loading increases, the Fe species bright spot signals in the corresponding mapping diagram increase. In addition, although the content of C element decreases, the distribution is more uniform. This is because the introduction of Fe changes the type and number of carbon-containing functional groups. At the same time, EDS quantitative analysis proves that the content of C is reduced. As a semi-quantitative analysis method, the content of elements in EDS is affected by the position of the selected material, indicating that the prepared composite material is a heterogeneous material.
[0048] Figure 3 The XRD patterns of BC, Fe@BC and 3Fe@BC are shown in Figure 2. Figure 3 It can be seen that in BC without iron addition, the (1 0 0) and (0 1 1) crystal planes of SiO2 were detected at 20.85° and 26.64°, respectively, and various crystal planes of NaAlSi3O8 were also found. With the progress of secondary calcination, the intensities of the characteristic peaks of SiO2 and NaAlSi3O8 of the two Fe-doped biochars increased, and a characteristic peak was found at a diffraction angle of 44.7° in Fe@BC, corresponding to Fe 0 (1 1 0) crystal plane; with the increase of Fe doping amount, in addition to the characteristic peak at a diffraction angle of 44.7°, there are also obvious characteristic peaks at 65.0° and 82.3° in 3Fe@BC, which correspond to Fe 0 The corresponding characteristic peaks can be compared with the results of Fe 0 The standard card (PDF#06-0696) corresponds to. 0 The formation of Fe is mainly due to the reduction of carbon combustion at high temperature. As the iron content increases, Fe 0The peaks will be enhanced and the crystal faces will increase. It can be concluded that by controlling the BC to be immersed in different concentrations of iron salts, the Fe 0 The amount of generation.
[0049] Figure 4 are TEM images of Fe@BC and 3Fe@BC. Figure 4 (a) is the TEM image of Fe@BC, where Fe 0 It appears on the BC surface in a spherical shape, with a small content, uniform dispersion, and no agglomeration. Figure 4 (b) is the TEM image of 3Fe@BC, where Fe 0 Agglomeration occurred, which may be due to the large amount of Fe loading. 0 Strong van der Waals forces are generated between the particles. Figure 4 In (c), the well-arranged lattice fringe spacing is observed to be 0.2457 nm, corresponding to Fe 0 The (1 1 0) crystal plane is consistent with the XRD results.
[0050] The adsorption types of BC, Fe@BC and 3Fe@BC were analyzed by N2 adsorption-desorption isotherms, and the specific surface areas, pore sizes and pore volumes of BC, Fe@BC and 3Fe@BC were calculated. Figure 5 And as shown in Table 1.
[0051] Tab 3.3 Specific surface area, pore size and pore volume of different samples
[0052]
[0053] from Figure 5(a) It can be seen that BC, Fe@BC and 3Fe@BC all show type IV isotherms, which indicates that there are multiple adsorption sites on the surface of the material. These sites may have different affinities for molecules. As the pressure increases, the number of adsorption sites increases, resulting in an increase in the adsorption amount. When all adsorption sites are occupied, the surface of the adsorbent begins to be saturated and the adsorption amount begins to decrease. In addition, BC, Fe@BC and 3Fe@BC all show H3 hysteresis loops. The H3 hysteresis loop is a characteristic phenomenon that appears in the type IV adsorption isotherm, that is, before the adsorption amount begins to decrease, the adsorption isotherm has a critical pressure point, at which time the adsorption amount no longer increases, and the adsorption isotherm presents a horizontal section. Previous studies have pointed out that the hysteresis loop that appears in the relative pressure range of 0.4 to 1.0 is attributed to the mesoporous effect. Therefore, it is speculated that BC, Fe@BC and 3Fe@BC are all mesoporous materials, which contain lamellar structures and irregular pore structures inside, which helps pollutants to diffuse rapidly on the Fe@BC surface. The specific surface areas of BC, Fe@BC and 3Fe@BC are 136.12, 116.44 and 79.54 m 2 / g. This shows that with the addition of Fe, the specific surface area of the material decreases. This may be because the newly added Fe particles gradually fill the pores of the carbon material, thereby reducing the original specific surface area of BC. Figure 5 (b) The pore size distribution is depicted. It is found that the pore sizes of BC, Fe@BC and 3Fe@BC are mainly distributed in the range of 2–20 nm. The pore volumes of BC, Fe@BC and 3Fe@BC are 0.1044, 0.1128 and 0.0719 cm, respectively. 3 / g.
[0054] FTIR further investigated the functional groups on the surfaces of BC, Fe@BC, and 3Fe@BC. As shown in Figure 6, for the BC material, at 3421 cm -1 The stretching vibration peak of -OH is at 3364 cm-1, while the stretching vibration peak of OH in Fe@BC occurs at 3364 cm-1. -1 1087cm -1 The bands near 794 cm correspond to the stretching vibration of -COOH. -1 The stretching vibration peak of 591cm is the Si–C or Si–O bond. -1 The absorption near 463 cm is usually associated with the stretching vibration of Si-O. -1 The presence of corresponds to Si–O–Si or Si–O–Al bonds. The functional groups of BC in 3Fe@BC are not obvious, which may be due to the large amount of Fe particles covering. FTIR analysis shows that the Fe@BC surface has abundant oxygen-containing functional groups, which is conducive to the adsorption and contact of PDS and TC on the Fe@BC surface.
[0055] In order to conduct an in-depth analysis of the chemical composition of BC, Fe@BC and 3Fe@BC and the valence state of surface elements, XPS was used for characterization. Figure 7 (a) shows the full XPS spectra of the three materials. It is worth noting that significant Fe 2p signals can be observed in the full spectra of Fe@BC and 3Fe@BC, which strongly proves that Fe has been successfully incorporated into BC, and the greater the loading, the more obvious the peak.
[0056] In addition, by Figure 7 (b) It can be seen that the Fe 2p of Fe@BC is mainly composed of Fe 2+ 2p 3 / 2 (709.6eV), Fe 2+ 2p 1 / 2 (723 eV) and Fe 3+ 2p 3 / 2 (712eV), Fe 3+ 2p 1 / 2 (725.33eV) consists of two groups of double peaks, and Fe is not fitted 0 The characteristic peak may be caused by Fe 0 The low content and easy oxidation result in the Fe 2+ and Fe 3+ This further verifies the successful doping of Fe.
[0057] Figure 8 The Raman spectra of BC, Fe@BC and 3Fe@BC are shown. -1 and 1580cm -1 At BC, Fe@BC and 3Fe@BC, obvious characteristic peaks appear, which reflect the defect degree and graphite structure of the materials respectively. By calculating the intensity ratio of these two peaks (I D / I G ), which can evaluate the degree of defects and graphitization of carbon materials. Specifically, I D / I G The higher the value, the more significant the defects of the material and the lower the degree of graphitization.
[0058] For BC, Fe@BC and 3Fe@BC, their I D / I G The values are 2.10, 2.41 and 2.19 respectively. This indicates that Fe doping increases the structural defect of BC, among which Fe@BC has the highest I D / I GThese defects can improve the electron transfer efficiency of Fe@BC to the substrate, thereby enhancing the catalytic reaction, indicating that Fe@BC has the best PDS activation performance.
[0059] Example 4 Experiment on TC degradation by activation of PDS using Fe-doped copper algae biochar
[0060] Take 100mL of 20mg / L tetracycline solution and add it to a 250mL beaker, then place the beaker on a magnetic stirrer. Add 0.004g of Fe@BC to it and darkly adsorb at 180rpm for 30min. Then, add 1mmol / L of potassium persulfate (PDS) to the mixed solution to start the catalytic reaction. During the reaction, samples were taken at time intervals of (0, 10, 20, 30, 40, 50, 60, 70, 80, 90min), and 2mL of samples were taken each time. The samples were filtered through a 0.22um filter membrane, and 1mL of methanol was added to stop the oxidation reaction. In addition, a comparative test of different catalyst systems (PDS, BC, Fe@BC, 3Fe@BC, BC+PDS, Fe@BC+PDS, 3Fe@BC+PDS) was set up to explore their effects on the catalytic reaction.
[0061] Analysis of catalytic performance of different systems
[0062] like Fig. 9 The ability of different systems to activate PDS to remove TC was compared. Fig. 9 (a) It can be seen that when only PDS exists, the mass concentration of TC remains almost unchanged, which reflects that the oxidation capacity of PDS itself is quite limited. In the presence of BC alone, the TC removal rate is less than 20%, indicating that BC itself has a very limited ability to activate PDS. In contrast, when PDS co-exists with Fe@BC and 3Fe@BC, the TC removal efficiency reaches 70% to 90%. It is worth noting that the adsorption rates of TC by BC, Fe@BC and 3Fe@BC are all less than 20%. Therefore, the main mechanism of Fe@BC activating PDS to remove TC is degradation rather than adsorption. Among them, the Fe@BC+PDS system exhibits the best catalytic performance, with a TC removal rate of 83.27% within 90 minutes, and the apparent rate constant (kobs) of TC in the Fe@BC+PDS system reaches 0.0250min. -1 , is the BC+PDS system (0.00041min -1 ) is 60.97 times ( Fig. 9 (c)). The results show that Fe-doped BC can promote the activation of PDS and effectively remove TC from the solution. In order to further study the reaction performance of the catalyst, Fe@BC with the best catalytic effect was selected for subsequent experimental research.
[0063] Effect of Fe@BC dosage
[0064] In order to optimize the degradation performance of Fe@BC+PDS system on TC, TC degradation experiments were carried out with different Fe@BC dosages. Fig.10 When the dosage of Fe@BC increased from 0.02 g / L to 0.04 g / L, the degradation rate of TC increased significantly from 71.35% to 82.75%, and the corresponding rate constant also increased from 0.021 min -1 Increase to 0.025min -1 (See Fig.10 (c)). This is because as the dosage of Fe@BC increases, the number of catalytic active sites of the reaction increases accordingly, thereby increasing the contact area between Fe@BC and TC, thereby enhancing the removal capacity of TC. However, when the dosage of Fe@BC further increases from 0.04 g / L to 0.08 g / L, the reaction rate constant kobs decreases slightly. This is because the concentration of PDS in the system is limited and is almost completely consumed within 10 minutes after the start of the reaction. Therefore, it does not bring a higher TC removal effect than when the dosage is 0.04 g / L. Taking all factors into consideration, the dosage of Fe@BC was set to 0.04 g / L for subsequent experiments.
[0065] Effect of PDS concentration
[0066] In addition, the effect of different PDS concentrations on TC removal was investigated under the same Fe@BC dosage conditions. Fig.11 As shown in (a), when the Fe@BC dosage is 0.04 g / L, the degradation efficiency of TC within 90 min is 59.28%, 78.37%, 83.27%, and 80.19% when the potassium persulfate (PDS) concentration is 0.1, 0.5, 1, and 2 mmol / L, respectively. As the PDS concentration increases from 0.1 mmol / L to 1 mmol / L, the corresponding rate constant increases from 0.0091 min -1 Increase to 0.0250min -1 (See Fig.11 (c)). This is because, when the mass concentration of PDS is low, the increase in its concentration will lead to the generation of more free radicals, but when the concentration of PDS increases to 2mmol / L, the Fe@BC+PDS system shows a slight inhibitory effect on the removal of TC. This is because when PDS reaches a certain concentration, the number of free radicals will not increase further due to the increase in PDS concentration. This may be attributed to the competitive inhibition effect when the mass concentration of PDS is high. Taking all factors into consideration, the PDS concentration was set to 1mmol / L for subsequent experiments.
[0067] Effect of TC initial mass concentration
[0068] Fig.12 The effect of the initial mass concentration of TC on the degradation of TC by Fe@BC activated PDS. When the initial mass concentration of TC was 10 mg / L, the degradation efficiency of TC was as high as 91.4% within 30 min. When the initial mass concentration of TC increased to 50 mg / L, the degradation efficiency dropped to 74.26%. It can be seen that the degradation rate of TC decreased with the increase of the initial mass concentration of TC, which is because the active sites of Fe@BC and PDS are limited. The results show that: without increasing the dosage, the smaller the initial mass concentration of TC, the fewer TC molecules, and a larger proportion of TC molecules occupy the active sites, so the degradation rate is higher.
[0069] Effect of initial temperature of TC solution
[0070] Fig.13 The effect of different temperatures on the degradation of TC by Fe@BC activated PDS. As the temperature increases from 15°C to 45°C, the degradation efficiency of TC by Fe@BC activated PDS is 83.27%, 85.25%, 90.2% and 96.43% within 90 minutes, respectively. As the temperature increases, the degradation rate of TC accelerates. This is because the increase in temperature will activate the activation of Fe@BC on PDS, thereby accelerating the degradation of TC.
[0071] Inorganic anion effects
[0072] Take 100mL of TC solution with a concentration of 20mg / L and add it to a 250mL beaker, then place the beaker on a magnetic stirrer. Add 0.004g of Fe@BC to it and darkly adsorb it at a speed of 180rpm for 30min. Then, add 1mmol / L of potassium persulfate (PDS) to the mixed solution to start the catalytic reaction. During the reaction, samples were taken at time intervals of (0, 10, 20, 30, 40, 50, 60, 70, 80, 90min), and 2mL of samples were taken each time. The samples were filtered through a 0.22um filter membrane, and 1mL of methanol was added to terminate the oxidation reaction. In addition, comparative experiments were set up with different catalyst systems (PDS, BC, Fe@BC, 3Fe@BC, BC+PDS, Fe@BC+PDS, 3Fe@BC+PDS), catalyst dosage (0.002, 0.004, 0.006, 0.008 g), PDS concentration (0.1, 0.5, 1, 2 mmol / L), TC concentration (10, 20, 30, 40, 50 mg / L), temperature (15, 25, 35, 45 °C), and coexisting anions (0.05 mol / L of KCl, K2SO4, KHCO3 and KH2PO4) to explore their effects on the catalytic reaction.
[0073] In order to evaluate the application effect of Fe@BC+PDS system in real wastewater, different anions (Cl - 、SO4 2- 、HCO3 - and H2PO4 - ) on TC degradation. Fig.14 As shown, the inhibition degree of various inorganic anions on TC removal is as follows: H2PO4 - >HCO3 - >SO4 2- >Cl-. The presence of Cl- partially inhibited the degradation performance of Fe@BC+PDS system for TC, and the degradation rate decreased by 15.35%. This may be due to the fact that Cl- consumed free radicals to produce Cl-·, ClOH-· and Cl2 - ·Waste oxidizing substances such as SO4 are added 2- After that, the degradation efficiency of TC dropped to 60.34%, which may be mainly due to SO4 2- The presence of SO4 ·- / SO4 2- The redox potential decreases. It is worth noting that in HCO3 - In the presence of HCO3, Fe@BC activated PDS only removed 41.23% of TC within 90 min, showing a significant inhibitory effect, which may be due to - SO4 produced by PDS ·- Reacts with OH to generate CO3 - , resulting in SO4 in the system ·- The reduction of ·OH and the decrease of TC degradation capacity of the system. - After that, the removal efficiency of TC dropped to 22.21%, which was due to the - Occupies the active center of Fe@BC and produces H2PO4 with low redox potential - ·.
[0074] TC degradation experiments show that under the reaction conditions of TC solution initial pH 4.6, initial temperature 45℃, Fe@BC dosage 0.04g / L, TC initial mass concentration 20mg / L and potassium persulfate (PDS) concentration 1mmol / L, the TC removal rate can be as high as 96% within 60min.
[0075] Finally, it should be noted that the above is only a specific embodiment of the present invention. Obviously, the present invention is not limited to the above embodiment, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. A method for preparing Fe-doped copper algae biochar, characterized in that: The following steps are involved: 1) Pretreatment of copper algae: soak and rinse the copper algae with deionized water until there is no obvious impurity, dry and crush, sieve, and obtain copper algae powder for later use; 2) Preparation of copper algae biochar: copper algae powder was placed in a square corundum crucible and calcined in a tube furnace. After calcination, it was cooled to room temperature, rinsed with deionized water until neutral, and dried to obtain copper algae biochar BC; 3) Preparation of Fe-doped copper algae biochar The copper algae biochar BC in step 2) is weighed, immersed in a FeCl3·6H2O solution, and stirred to allow the copper algae biochar BC to fully absorb the iron salt. Then, the BC absorbing different concentrations of iron salts is placed in a drying oven to dry to obtain a precursor of the mixed material; then, the precursor is transferred to a square corundum crucible, placed in a tubular furnace, and calcined to obtain Fe-doped copper algae biochar Fe@BC.
2. The method for preparing Fe-doped copper algae biochar according to claim 1, characterized in that: The sieving in step 1) is 100 mesh.
3. The method for preparing Fe-doped copper algae biochar according to claim 1, characterized in that: The calcination procedure in the step 2) is: introduce 99.999% high-purity N2 at a flow rate of 100 mL / min, and ventilate for 30 minutes to exhaust the air in the furnace; increase the temperature from room temperature to 200°C at a heating rate of 10°C / min, maintain for 30 minutes, and then increase the temperature from 200°C to 700°C at the same heating rate, and maintain for 120 minutes.
4. The method for preparing Fe-doped copper algae biochar according to claim 1, characterized in that: The cooling after calcination in step 2) is as follows: reducing the temperature to 300° C. at a rate of 10° C. / min, turning off the tube furnace and N2, and cooling naturally to room temperature.
5. The method for preparing Fe-doped copper algae biochar according to claim 1, characterized in that: The concentration of the FeCl3·6H2O solution in step 3) is 0.03 mol / L-0.3 mol / L.
6. The method for preparing Fe-doped copper algae biochar according to claim 1, characterized in that: In the step 3), the weight volume ratio of copper algae biochar BC to FeCl3·6H2O solution is 1g:100ml.
7. The method for preparing Fe-doped copper algae biochar according to claim 1, characterized in that: The calcination procedure in the step 3) is to use N2 with a flow rate of 100 mL / min to purge the residual air in the furnace, then set the heating rate to 5°C / min, raise the carbonization temperature to 900°C, carbonize at a constant temperature for 2 hours, reduce the temperature to 300°C at a cooling rate of 5°C / min, then turn off the tube furnace and wait for the sample to cool to room temperature.
8. Fe-doped copper algae biochar is prepared by the method according to any one of claims 1 to 7.
9. Use of the Fe-doped copper algae biochar as claimed in claim 8 in degrading tetracycline TC.
10. The use of Fe-doped copper algae biochar in the degradation of tetracycline TC as claimed in claim 9, wherein the conditions for degrading tetracycline are: the initial pH of the TC solution is 4.6, the initial temperature is 45°C, the dosage of Fe-doped copper algae biochar Fe@BC is 0.04 g / L, the initial mass concentration of TC is 20 mg / L, and the PDS concentration is 1 mmol / L. Preferably, the PDS is potassium persulfate.
Citation Information
Patent Citations
Preparation method of sargassum horneri matrix activated carbon
CN103408011A
Magnetic nitrogen-doped biochar composite material as well as preparation method and application thereof
CN115608395A
Seaweed biochar ZnO photocatalyst and preparation method thereof
CN117753401A
Cited By
Preparation method and application of biochar composite material
CN120205144A
Preparation method and application of biochar composite material
CN120205144B