Preparation method and application of carbon-supported cobalt ferrite catalyst

By preparing a carbon-supported cobalt ferrite catalyst, the problem of low activation efficiency of CoFe2O4 catalyst is solved, the activation efficiency of peroxymonosulfate and the oxidation ability of organic matter are improved, and the effect of efficient degradation of pollutants is achieved.

CN118807749APending Publication Date: 2024-10-22ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410835613.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The CoFe2O4 catalyst has low efficiency during the activation process of peroxymonosulfate and is easily deactivated, resulting in a reduced electron transfer rate and inability to effectively degrade antibiotics and other pollutants.

Method used

By preparing a carbon-supported cobalt ferrite catalyst, plant tissues and metal-organic frameworks are calcined in an oxygen atmosphere to form amorphous carbon and CoFe2O4 with many defects, which enhances the activation efficiency of the catalyst for peroxymonosulfate.

Benefits of technology

It improves the activation efficiency of peroxymonosulfate by CoFe2O4, enhances the oxidation ability of organic matter, and achieves efficient degradation of antibiotics and other pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807749A_ABST
    Figure CN118807749A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a carbon-supported cobalt ferrite catalyst, and the preparation method of the carbon-supported cobalt ferrite catalyst comprises the following steps: preparing a mixed solution in which divalent cobalt salt and trivalent iron salt are dissolved, and adding ferricyanide into the mixed solution to obtain a metal organic framework material suspension; adding a plant tissue body into the metal organic framework material suspension to obtain a mixed solution; carrying out solid-liquid separation on the mixed solution, and collecting solids; and calcining the solid matter in an aerobic atmosphere to decompose the metal organic framework material and carbonize the plant tissue body to obtain the carbon-supported cobalt ferrite catalyst. The carbon-supported cobalt ferrite catalyst prepared by the invention has high activation efficiency on peroxymonosulfate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of environmental protection, and in particular to the degradation of pollutants. Background Art

[0002] In the field of water environment remediation, PMS (peroxymonosulfate) activation technology is an advanced oxidation technology (AOPs) that can quickly degrade pollutants such as antibiotics at room temperature and pressure. Transition metal catalysis is the mainstream PMS activation method. Transition metals can transfer electrons with PMS, making PMS (HSO5 - ) breaks the O–O bond in the ions, generating active oxygen free radicals such as hydroxyl radicals (·OH), sulfate radicals (SO4· - ), etc., thereby degrading organic matter.

[0003] CoFe2O4 has been widely used for peroxymonosulfate (PMS) activation due to its high catalytic activity and strong Co–Fe bond. However, CoFe2O4 has the problems of easy particle agglomeration, surface passivation, metal cycle interruption and ion leaching, which makes it easy to deactivate, which seriously inhibits the electron transfer rate and thus reduces its activation efficiency for PMS. In order to solve the problem of low activation efficiency of CoFe2O4, the existing technology loads CoFe2O4 onto carbon carriers such as carbon nanotubes and graphene to avoid the problem of easy deactivation of CoFe2O4, but the catalytic activation efficiency of CoFe2O4 is still not ideal. Summary of the invention

[0004] The embodiments of the present application provide a preparation method and application of a carbon-supported cobalt ferrite catalyst to solve the technical problem of low activation efficiency of CoFe2O4 for peroxymonosulfate.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing a carbon-supported cobalt ferrite catalyst, the method for preparing the carbon-supported cobalt ferrite catalyst comprising the following steps:

[0006] A mixed solution containing a divalent cobalt salt and a trivalent iron salt is prepared, and ferrocyanide is added to the mixed solution to obtain a metal organic framework material suspension;

[0007] adding plant tissue to the metal organic framework material suspension to obtain a mixed solution;

[0008] Performing solid-liquid separation on the mixed liquid to collect solids;

[0009] The solid matter is calcined in an oxygen atmosphere to decompose the metal organic framework material and carbonize the plant tissue to obtain a carbon-supported cobalt ferrite catalyst.

[0010] In some embodiments of the present application, plant tissues are added to the metal-organic framework material suspension, and a pore-increasing agent is also added to the metal-organic framework material suspension.

[0011] In some embodiments of the present application, the pore-increasing agent is at least one of bicarbonate and citrate.

[0012] In some embodiments of the present application, the ratio of the weight of the pore opener to the dry weight of the plant tissue is 1:1.8-2.2.

[0013] In some embodiments of the present application, in the metal organic framework material suspension, Co 2+ and Fe 3+ The molar ratio is 6:2 to 9; and / or,

[0014] Co 2+ and Fe 3+ Total molar amount and [Fe(CN)6] 3- The molar ratio is 3:2.

[0015] In some embodiments of the present application, in the mixed solution, Co 2+ and Fe 3+ The ratio of the total mass of the plant tissue to the dry weight of the plant tissue is 1:1-8.

[0016] In some embodiments of the present application, the calcining of the solid in an oxygen atmosphere comprises the following steps:

[0017] The solid is heated to 400-800° C. at a heating rate of 2-10° C. / min in air for 1-4 hours.

[0018] In some embodiments of the present application, the solid-liquid separation method is one of filtration and centrifugation.

[0019] In some embodiments of the present application, the plant tissue is straw powder.

[0020] In a second aspect, an embodiment of the present application provides an application of a carbon-supported cobalt ferrite catalyst, wherein the carbon-supported cobalt ferrite catalyst is a carbon-supported cobalt ferrite catalyst prepared by the preparation method of the carbon-supported cobalt ferrite catalyst described in any embodiment of the first aspect, and the carbon-supported cobalt ferrite catalyst is used for the activation of peroxymonosulfate.

[0021] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0022] The preparation method of the carbon-supported cobalt ferrite catalyst provided in the embodiment of the present application comprises: 2+ and Fe 3+The metal-organic framework and plant tissue are calcined to carbonize the plant tissue to form amorphous carbon. During this process, the metal-organic framework collapses and forms CoFe2O4 with a large number of defects. The amorphous carbon can also promote the surface adsorption of the catalyst on PMS and act as an electron medium to achieve direct oxidation of organic matter, which makes CoFe2O4 have a high activation efficiency for peroxymonosulfate. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0025] Figure 1 It is a schematic flow chart of the preparation method of the carbon-supported cobalt ferrite catalyst provided in the examples of the present application.

[0026] Figure 2 This is the XRD spectrum of the metal organic framework obtained in Example 1 of the present application.

[0027] Figure 3 It is a pore size distribution diagram of the carbon-supported cobalt ferrite catalyst obtained in Example 1 of the present application and the cobalt ferrite catalyst obtained in Comparative Example 1.

[0028] Figure 4 It is the infrared spectra of the carbon-supported cobalt ferrite catalyst obtained in Example 1 of the present application, the cobalt ferrite catalyst obtained in Comparative Example 1, and the amorphous carbon obtained in Comparative Example 2.

[0029] Figure 5 It is a surface potential distribution diagram of a complete carbon structure, a carbon structure with defects, a carbon structure with a C=O group, and a carbon structure with a C–O group.

[0030] Figure 6 This is a SEM image of the carbon-supported cobalt ferrite catalyst obtained in Example 1 of the present application.

[0031] Figure 7 This is a SEM image of the cobalt ferrite catalyst obtained in Comparative Example 1 of the present application. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0033] Unless otherwise specified, the terms used herein should be understood as commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. In the event of a conflict, this specification takes precedence.

[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0035] Currently, CoFe2O4 has a technical problem of low activation efficiency for peroxymonosulfate.

[0036] The technical solution provided by the embodiments of the present application is to solve the above technical problems, and the overall idea is as follows:

[0037] In a first aspect, an embodiment of the present application provides a method for preparing a carbon-supported cobalt ferrite catalyst, the method for preparing the carbon-supported cobalt ferrite catalyst comprising the following steps:

[0038] S1: preparing a mixed solution containing a divalent cobalt salt and a trivalent iron salt, and adding ferrocyanide to the mixed solution to obtain a metal organic framework material suspension;

[0039] S2: adding plant tissue to the metal organic framework material suspension to obtain a mixed solution;

[0040] S3: performing solid-liquid separation on the mixed liquid to collect solids;

[0041] S4: calcining the solid in an oxygen atmosphere to decompose the metal organic framework material and carbonize the plant tissue to obtain a carbon-supported cobalt ferrite catalyst.

[0042] It is easy to understand that the metal organic framework is a face-centered cubic structure. The solid contains the metal organic framework and the plant tissue. During calcination, in an oxygen atmosphere, the C and N elements form gases and escape, and the O element reacts with the Co 2+ and Fe 3+CoFe2O4 is formed. The face-centered cubic structure of the metal organic framework collapses during the calcination process, resulting in more defects in CoFe2O4, forming active centers that can activate PMS. Plant tissues are thermally decomposed during the calcination process to form amorphous carbon. In an oxygen atmosphere, oxygen-containing groups are also formed on the surface of amorphous carbon, which makes the amorphous carbon have a large number of intrinsic carbon defect sites and oxygen-containing functional groups, thereby inducing the metal organic framework to produce more active centers during the collapse process. In addition, the defects and oxygen-containing functional groups in amorphous carbon will change the original carbon structure, disrupt the originally uniform charge distribution, and increase the potential around the defect sites and oxygen-containing functional groups, which can promote the catalyst's surface adsorption of PMS and act as an electron medium to achieve direct oxidation of organic matter.

[0043] When the carbon-supported cobalt ferrite catalyst is activated by PMS, on the one hand, PMS is activated by low-valent cobalt, low-valent iron, oxygen-containing functional groups and structural defects in the CoFe2O4 / C composite catalyst to generate reactive oxygen species (ROS) to degrade organic pollutants; on the other hand, PMS molecules form active PMS molecules (PMS*) on the surface of the CoFe2O4 / C composite catalyst with unstable electronic configuration, ultimately achieving efficient activation of PMS.

[0044] This application is based on the 2+ and Fe 3+ The metal-organic framework and plant tissue are calcined to carbonize the plant tissue to form amorphous carbon. During this process, the metal-organic framework collapses and forms CoFe2O4 with a large number of defects. The amorphous carbon can also promote the surface adsorption of the catalyst on PMS and act as an electron medium to achieve direct oxidation of organic matter, which makes CoFe2O4 have a high activation efficiency for peroxymonosulfate.

[0045] In some embodiments of the present application, plant tissues are added to the metal-organic framework material suspension, and a pore-increasing agent is also added to the metal-organic framework material suspension.

[0046] It is easy to understand that the pore-increasing agent can increase the porosity of the carbon-supported cobalt ferrite catalyst, thereby increasing its contact area with peroxymonosulfate, thereby increasing the activation efficiency.

[0047] In some embodiments of the present application, the pore-increasing agent is at least one of bicarbonate and citrate.

[0048] As an example, the pore-enhancing agent may be sodium bicarbonate, potassium bicarbonate, sodium citrate, potassium citrate or the like.

[0049] In some embodiments of the present application, the ratio of the weight of the pore opener to the dry weight of the plant tissue is 1:1.8-2.2.

[0050] As an example, the ratio of the weight of the pore opener to the dry weight of the plant tissue can be 1:1.8, 1:1.9, 1:2.0, 1:2.1, or 1:2.2.

[0051] In some embodiments of the present application, in the metal organic framework material suspension, Co 2+ and Fe 3+ The molar ratio is 6:2 to 9; and / or,

[0052] Co 2+ and Fe 3+ Total molar amount and [Fe(CN)6] 3- The molar ratio is 3:2.

[0053] In some embodiments of the present application, in the mixed solution, Co 2+ and Fe 3+ The ratio of the total mass of the plant tissue to the dry weight of the plant tissue is 1:1-8.

[0054] As an example, Co 2+ and Fe 3+ The ratio of the total mass of the plant to the dry weight of the plant tissue can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, or 1:8.

[0055] In some embodiments of the present application, the calcining of the solid in an oxygen atmosphere comprises the following steps:

[0056] S41: In air, heat the solid to 400-800° C. at a heating rate of 2-10° C. / min for 1-4 hours.

[0057] In some embodiments of the present application, the solid-liquid separation method is one of filtration and centrifugation.

[0058] In some embodiments of the present application, the plant tissue is straw powder.

[0059] In a second aspect, an embodiment of the present application provides an application of a carbon-supported cobalt ferrite catalyst, wherein the carbon-supported cobalt ferrite catalyst is a carbon-supported cobalt ferrite catalyst prepared by the preparation method of the carbon-supported cobalt ferrite catalyst described in any embodiment of the first aspect, and the carbon-supported cobalt ferrite catalyst is used for the activation of peroxymonosulfate.

[0060] It is easy to understand that the carbon-supported cobalt ferrite catalyst is used in the following scenario: using peroxymonosulfate as an oxidant to oxidize organic matter in sewage.

[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0062] Example 1

[0063] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:1, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0064] Add straw powder and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:1, the mass ratio of sodium bicarbonate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0065] The suspension was centrifuged to remove the solvent to obtain a solid, which was washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C for 2 hours, and then naturally cooled to room temperature to obtain Co3Fe1O x / C composite catalyst, that is, carbon-supported cobalt ferrite catalyst.

[0066] Dissolve BPA (bisphenol A) in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0±0.1;

[0067] Add Co3Fe1O to BPA solution x / C composite catalyst and peroxymonosulfate, shake well quickly and place in a shaker, the catalyst dosage is 0.1g / L, the oxidant dosage is 0.45mmol / L;

[0068] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0069] At 10, 20 and 30 min, the BPA removal rates were 42.6%, 83.7% and 100%, respectively.

[0070] A portion of the metal organic framework material was collected for XRD detection, and the detection results were as follows: Figure 2 By comparing with the PDF standard card, it can be determined that the prepared metal organic framework material is a Prussian blue compound.

[0071] Example 2

[0072] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0073] Add straw powder and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:1, the mass ratio of sodium bicarbonate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0074] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0075] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0076] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0077] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0078] Figure 1The scanning electron microscope image of the CoFe2O4 / C composite catalyst is shown, and it can be seen that the CoFe2O4 / C composite catalyst has a rougher surface than CoFe2O4. At 10, 20, 30 and 40 min, the BPA removal rates were 35.9%, 64.3%, 88.9% and 99.1%, respectively.

[0079] Example 3

[0080] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 2:3, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0081] Add straw powder and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:1, the mass ratio of sodium bicarbonate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0082] The suspension was centrifuged to remove the solvent to obtain a solid, which was washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C for 2 hours, and then naturally cooled to room temperature to obtain Co2Fe3O x / C composite catalyst, that is, carbon-supported cobalt ferrite catalyst.

[0083] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0084] Add Co2Fe3O to BPA solution x / C composite catalyst and peroxymonosulfate, shake well quickly and place in a shaker, the catalyst dosage is 0.1g / L, the oxidant dosage is 0.45mmol / L;

[0085] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0086] At 10, 20, 30 and 40 min, the BPA removal rates were 33.7%, 57.6%, 79.2% and 89.4%, respectively.

[0087] Example 4

[0088] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0089] Add straw powder and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of and the straw powder is 1:2, the mass ratio of sodium bicarbonate and and the straw powder is 1:2, and ultrasonic shaking and mixing are performed to obtain a suspension;

[0090] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0091] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0092] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0093] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0094] At 10, 20, 30 and 40 min, the BPA removal rates were 42.5%, 77.4%, 97.2% and 100%, respectively.

[0095] Example 5

[0096] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0097] Add straw powder and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium bicarbonate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0098] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0099] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0100] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0101] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0102] At 10, 20 and 30 min, the BPA removal rates were 58.2%, 95.7% and 100%, respectively.

[0103] Example 6

[0104] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0105] Add straw powder and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+The total mass ratio of to the straw powder is 1:8, the mass ratio of sodium bicarbonate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0106] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0107] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0108] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0109] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0110] At 10, 20 and 30 min, the BPA removal rates were 53.5%, 92.7% and 100%, respectively.

[0111] Example 7

[0112] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0113] Add straw powder and sodium citrate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium citrate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0114] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0115] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 22.5 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0116] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0117] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0118] At 10 and 20 min, the BPA removal rates were 94.3% and 100%, respectively.

[0119] Example 8

[0120] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0121] Add straw powder and sodium citrate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium citrate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0122] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0123] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 90 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0124] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0125] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0126] At 10, 20, 30 and 40 min, the BPA removal rates were 50.5%, 83.8%, 97.7% and 99.7%, respectively.

[0127] Example 9

[0128] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0129] Add straw powder and sodium citrate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium citrate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0130] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0131] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 180 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0132] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0133] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0134] At 10, 20, 30 and 40 min, the BPA removal rates were 50.5%, 83.8%, 97.7% and 99.7%, respectively.

[0135] Example 10

[0136] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0137] Add straw powder and sodium citrate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium citrate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0138] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0139] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0140] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake quickly and place in a shaker, the catalyst dosage is 0.1g / L, the oxidant dosage is 0.225mmol / L;

[0141] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0142] At 10, 20 and 30 min, the BPA removal rates were 68.1%, 95.8% and 100%.

[0143] Embodiment 11

[0144] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0145] Add straw powder and sodium citrate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium citrate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0146] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0147] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0148] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.90 mmol / L.

[0149] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0150] At 10, 20 and 30 min, the BPA removal rates were 77.2%, 99.6% and 100%.

[0151] Example 12

[0152] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0153] Add straw powder and sodium citrate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of sodium citrate to the straw powder is 1:2, and ultrasonic shaking is used to mix to obtain a suspension;

[0154] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0155] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0156] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 1.80 mmol / L.

[0157] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0158] At 10, 20 and 30 min, the BPA removal rates were 73.2%, 98.9% and 100%.

[0159] Embodiment 13

[0160] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0161] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0162] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0163] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0164] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.05 g / L and the oxidant dosage is 0.45 mmol / L.

[0165] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0166] At 10, 20, 30 and 40 min, the BPA removal rates were 36.6%, 64.5%, 86.9% and 97.5%, respectively.

[0167] Embodiment 14

[0168] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0169] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0170] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0171] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0172] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.2 g / L and the oxidant dosage is 0.45 mmol / L.

[0173] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0174] At 10 and 20 min, the BPA removal rates were 89.3% and 100%, respectively.

[0175] Embodiment 15

[0176] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0177] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0178] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0179] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0180] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.4 g / L and the oxidant dosage is 0.45 mmol / L.

[0181] Samples were taken after 0, 5, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0182] At 5 and 10 min, the BPA removal rates were 88.6% and 100%, respectively.

[0183] Example 16

[0184] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0185] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0186] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0187] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 2.0 ± 0.1;

[0188] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0189] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0190] At 10, 20, 30 and 40 min, the BPA removal rates were 41.3%, 74.2%, 90.1% and 100%, respectively.

[0191] Embodiment 17

[0192] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0193] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0194] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0195] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 4.0 ± 0.1;

[0196] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0197] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0198] At 10, 20 and 30 min, the BPA removal rates were 59.0%, 93.5% and 100%, respectively.

[0199] Embodiment 18

[0200] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0201] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0202] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0203] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 10.0±0.1;

[0204] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0205] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0206] At 10, 20 and 30 min, the BPA removal rates were 75.3%, 99.4% and 100%, respectively.

[0207] Embodiment 19

[0208] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0209] Add straw powder and a pore-increasing agent to the metal organic framework material suspension, wherein the pore-increasing agent is a mixture of sodium bicarbonate and potassium citrate in a mass ratio of 1:1, 2+ and Fe 3+ The total mass ratio of to the straw powder is 1:4, the mass ratio of the pore-increasing agent to the straw powder is 1:2, and ultrasonic oscillation is used to mix to obtain a suspension;

[0210] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 / C composite catalyst, i.e., a carbon-supported cobalt ferrite catalyst.

[0211] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 12.0 ± 0.1;

[0212] Add CoFe2O4 / C composite catalyst and peroxymonosulfate to the BPA solution, shake well quickly and place in a shaker. The catalyst dosage is 0.1 g / L and the oxidant dosage is 0.45 mmol / L.

[0213] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0214] At 10, 20, 30 and 40 min, the BPA removal rates were 66.4%, 89.7%, 95.3% and 100%, respectively.

[0215] Comparative Example 1

[0216] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:2, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0217] The metal organic framework material suspension is placed in a muffle furnace and calcined at 600°C at a heating rate of 10°C / min. After maintaining for 2 hours, it is naturally cooled to room temperature to obtain a CoFe2O4 catalyst, namely a cobalt ferrite catalyst.

[0218] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0219] Add CoFe2O4 catalyst and peroxymonosulfate to the BPA solution, shake quickly and place in a shaker, the catalyst dosage is 0.1g / L, and the oxidant dosage is 0.45mmol / L;

[0220] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0221] At 40 minutes, the BPA removal rate was less than 46%.

[0222] Comparative Example 2

[0223] The straw powder was placed in a muffle furnace and calcined at 600°C at a heating rate of 10°C / min for 2 hours, and then naturally cooled to room temperature to obtain amorphous carbon.

[0224] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0225] Add amorphous carbon and peroxymonosulfate to the BPA solution, shake quickly and place in a shaker, the amount of amorphous carbon added is 0.1 g / L, and the amount of oxidant added is 0.45 mmol / L;

[0226] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0227] At 40 minutes, the BPA removal rate was less than 16%.

[0228] Comparative Example 3

[0229] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:1, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0230] Graphite powder and sodium bicarbonate were added to the metal organic framework suspension. 2+ and Fe 3+ The total mass ratio of the total mass of the carbon dioxide to the straw powder is 1:1, and the mass ratio of the sodium bicarbonate to the graphite powder is 1:2, and ultrasonic vibration is used to mix to obtain a suspension;

[0231] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours under a nitrogen atmosphere, it is naturally cooled to room temperature to obtain a CoFe / GP composite catalyst, i.e., a graphite powder-supported cobalt-iron catalyst.

[0232] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0233] Add CoFe / GP composite catalyst and peroxymonosulfate to the BPA solution, shake quickly and place in a shaker, the catalyst dosage is 0.1 g / L, and the oxidant dosage is 0.45 mmol / L;

[0234] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0235] At 10, 20, 30 and 40 min, the BPA removal rates were 23.6%, 39.8%, 50.7% and 61.1%, respectively.

[0236] Comparative Example 4

[0237] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co 2+ and Fe 3+ The molar ratio of Co was 3:1, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0238] Add carbon nanotubes and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The mass ratio of the total mass of and the straw powder is 1:1, and the mass ratio of sodium bicarbonate and and the carbon nanotubes is 1:2, and ultrasonic shaking and mixing are performed to obtain a suspension;

[0239] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours under a nitrogen atmosphere, it is naturally cooled to room temperature to obtain a CoFe / CN composite catalyst, i.e., a carbon nanotube-supported cobalt-iron catalyst.

[0240] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0241] Add CoFe / CN composite catalyst and peroxymonosulfate to the BPA solution, shake quickly and place in a shaker, the catalyst dosage is 0.1 g / L, and the oxidant dosage is 0.45 mmol / L;

[0242] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0243] At 10, 20, 30 and 40 min, the BPA removal rates were 19.8%, 33.2%, 42.9% and 50.1%, respectively.

[0244] Comparative Example 5

[0245] Weigh cobalt nitrate hexahydrate and ferric nitrate nonahydrate and dissolve them in deionized water to control Co2+ and Fe 3+ The molar ratio of Co was 3:1, and the mixture was uniformly mixed to obtain a mixed solution. The mixed solution was placed on a magnetic stirrer for stirring, and a molar amount of Co 2+ and Fe 3+ 2 / 3 of the total molar amount of potassium ferrocyanide solution is continuously stirred to obtain a metal organic framework material suspension;

[0246] Add graphene and sodium bicarbonate to the metal organic framework suspension, Co 2+ and Fe 3+ The total mass ratio of the total mass of the graphene to the straw powder is 1:1, and the mass ratio of the sodium bicarbonate to the graphene is 1:2, and ultrasonic vibration is used to mix to obtain a suspension;

[0247] The suspension is centrifuged to remove the solvent to obtain a solid, and the solid is washed and dried, and then placed in a muffle furnace at a heating rate of 10°C / min and a calcination temperature of 600°C. After maintaining for 2 hours under a nitrogen atmosphere, it is naturally cooled to room temperature to obtain a CoFe / G composite catalyst, i.e., a graphene-supported cobalt-iron catalyst.

[0248] Dissolve BPA in deionized water to prepare a BPA solution with a BPA concentration of 45 μmol / L. Use hydrochloric acid and sodium hydroxide solution to adjust the pH of the BPA solution to 7.0 ± 0.1;

[0249] Add CoFe / G composite catalyst and peroxymonosulfate to the BPA solution, shake quickly and place in a shaker, the catalyst dosage is 0.1 g / L, and the oxidant dosage is 0.45 mmol / L;

[0250] Samples were taken after 0, 10, 20, 30 and 40 min of reaction, and an equal volume of methanol was added. After mixing evenly, the mixture was filtered and the BPA solubility was detected by HPLC equipped with a C8 column at a detection wavelength of 278 nm.

[0251] At 10, 20, 30 and 40 min, the BPA removal rates were 31.6%, 54.9%, 70.7% and 88.3%, respectively.

[0252] Related experiments and effect data:

[0253] The carbon-supported cobalt ferrite catalyst obtained in Example 1 and the cobalt ferrite catalyst obtained in Comparative Example 1 were tested for BET specific surface area. The test results are as follows: Figure 3 . Figure 3 The pore size distribution of the cobalt ferrite catalyst obtained in Comparative Example 1 is centered at 14.68 nm and the volume is 0.23 cm 3 / g, the pore size distribution peaks of the carbon-supported cobalt ferrite catalyst obtained in Example 1 are located at 3.26nm and 22.41nm, respectively, and the cumulative pore volume is 0.39cm 3 / g, which is significantly higher than that of Comparative Example 1. This indicates that the carbon-supported cobalt ferrite catalyst obtained in Example 1 has more pore structures and more contact sites with PMS, which can enhance the effective utilization of the catalyst active sites.

[0254] The carbon-supported cobalt ferrite catalyst obtained in Example 1, the cobalt ferrite catalyst obtained in Comparative Example 1, and the amorphous carbon obtained in Comparative Example 2 were subjected to infrared spectroscopy analysis. The obtained infrared spectra are shown in FIG. Figure 4 . Figure 4 This shows that the carbon-supported cobalt ferrite catalyst obtained in Example 1 and the amorphous carbon obtained in Comparative Example 2 both have C=O at 1694 cm -1 The characteristic absorption peaks at 1044 cm -1 This indicates that the carbon carrier of the carbon-supported cobalt ferrite catalyst obtained in Example 1 and the amorphous carbon obtained in Comparative Example 2 have undergone a certain degree of oxidation on their surfaces, forming oxygen-containing functional groups that enhance the catalytic efficiency.

[0255] Based on the DFT theory, the surface potential distribution diagrams of the complete carbon structure, the carbon structure with defects, the carbon structure with C=O groups, and the carbon structure with C–O groups are drawn respectively, such as Figure 5 . Figure 5 This shows that after introducing defects and oxygen-containing functional groups into the carbon structure, the carbon structure changes, disrupting the originally uniform charge distribution and increasing the potential around defect sites and oxygen-containing functional groups, which can promote the catalyst's surface adsorption of PMS and act as an electron medium to achieve direct oxidation of organic matter.

[0256] The carbon-supported cobalt ferrite catalyst obtained in Example 1 and the cobalt ferrite catalyst obtained in Comparative Example 1 were observed by scanning electron microscopy (SEM). Figure 6 This is the SEM image of the carbon-supported cobalt ferrite catalyst obtained in Example 1. Figure 7 This is the SEM image of the cobalt ferrite catalyst obtained in Comparative Example 1. Figure 6 and Figure 7 It can be clearly found that due to the presence of the carrier formed by carbonization of straw powder, the particles of the carbon-supported cobalt ferrite catalyst obtained in Example 1 are significantly smaller than the particles of the cobalt ferrite catalyst obtained in Comparative Example 1, which means that it has a larger specific surface area and more contact sites with PMS.

[0257] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0258] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present application specification, the terms "including", "comprising", etc. refer to "including but not limited to". Moreover, the terms "including", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "including..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. For the association relationship of more than three associated objects described by "and / or", it means that any one of these three associated objects can exist alone, or any at least two of them exist at the same time. For example, for A, and / or B, and / or C, it can be represented that any one of A, B, and C exists alone, or any two of them exist at the same time, or three of them exist at the same time. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single (individual) or plural (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, wherein a, b, and c can be single or multiple, respectively.

[0259] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A method for preparing a carbon-supported cobalt ferrite catalyst, characterized in that: The preparation method of the carbon-supported cobalt ferrite catalyst comprises the following steps: A mixed solution containing a divalent cobalt salt and a trivalent iron salt is prepared, and ferrocyanide is added to the mixed solution to obtain a metal organic framework material suspension; adding plant tissue to the metal organic framework material suspension to obtain a mixed solution; Performing solid-liquid separation on the mixed liquid to collect solids; The solid matter is calcined in an oxygen atmosphere to decompose the metal organic framework material and carbonize the plant tissue to obtain a carbon-supported cobalt ferrite catalyst.

2. The method for preparing a carbon-supported cobalt ferrite catalyst according to claim 1, characterized in that: Plant tissues are added to the metal organic framework material suspension, and a pore increasing agent is also added to the metal organic framework material suspension.

3. The method for preparing the carbon-supported cobalt ferrite catalyst according to claim 2, characterized in that: The pore-increasing agent is at least one of bicarbonate and citrate.

4. The method for preparing the carbon-supported cobalt ferrite catalyst according to claim 3, characterized in that: The ratio of the weight of the pore-enhancing agent to the dry weight of the plant tissue is 1:1.8-2.

2.

5. The method for preparing a carbon-supported cobalt ferrite catalyst according to claim 1, characterized in that: In the metal organic framework material suspension, Co 2+ and Fe 3+ The molar ratio is 6:2 to 9; and / or, Co 2+ and Fe 3+ Total molar amount and [Fe(CN)6] 3- The molar ratio is 3:

2.

6. The method for preparing the carbon-supported cobalt ferrite catalyst according to claim 5, characterized in that: In the mixed solution, Co 2+ and Fe 3+ The ratio of the total mass of the plant tissue to the dry weight of the plant tissue is 1:1-8.

7. The method for preparing a carbon-supported cobalt ferrite catalyst according to claim 1, characterized in that: The step of calcining the solid in an oxygen atmosphere comprises the following steps: The solid is heated to 400-800° C. at a heating rate of 2-10° C. / min in air for 1-4 hours.

8. The method for preparing a carbon-supported cobalt ferrite catalyst according to claim 1, characterized in that: The solid-liquid separation method is one of filtration and centrifugation.

9. The method for preparing a carbon-supported cobalt ferrite catalyst according to claim 1, characterized in that: The plant tissue is straw powder.

10. An application of a carbon-supported cobalt ferrite catalyst, characterized in that: The carbon-supported cobalt ferrite catalyst is a carbon-supported cobalt ferrite catalyst prepared by the preparation method of the carbon-supported cobalt ferrite catalyst according to any one of claims 1 to 9, and the carbon-supported cobalt ferrite catalyst is used for the activation of peroxymonosulfate.

Citation Information

Patent Citations

  • Method for preparing tricobalt tetraoxide nanosheet by double confinements of MOF-Co and biological template

    CN110357172A

  • Preparation method and application of ferrocobalt oxide heterogeneous Fenton-like catalyst with hollow frame structure

    CN115970695A

  • Preparation method and application of hydrothermal carbon loaded cobalt ferrite composite material

    CN116099536A