Carbon dot doped Co3O4 catalyst as well as preparation method and application thereof

The carbon dot-doped Co3O4 catalyst formed by calcination solves the problems of low efficiency and insufficient microwave response of the Co3O4 catalyst in NaBH4 hydrolysis to produce hydrogen, achieves efficient hydrogen generation and microwave response intensity, and significantly improves the performance of the catalyst.

CN118807750APending Publication Date: 2024-10-22NINGBO INST OF TECH ZHEJIANG UNIV ZHEJIANG +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410859367.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The Co3O4 catalyst has low efficiency and insufficient response to microwaves in NaBH4 hydrolysis to produce hydrogen, and cannot effectively increase the reaction rate.

Method used

By mixing carbon raw materials with cobalt salts, adding alkaline solution and then calcining, a carbon dot-doped Co3O4 catalyst is formed. The calcining temperature is controlled at 300-900°C to increase active sites and conductivity, and improve microwave response.

Benefits of technology

Significantly improve the rate and catalytic efficiency of NaBH4 hydrolysis to produce hydrogen. The carbon dot-doped Co3O4 catalyst can respond efficiently under microwave conditions, and the hydrogen production rate reaches 7107mL/min/g, which is much higher than that of undoped Co3O4 of 1576mL/min/ g.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807750A_ABST
    Figure CN118807750A_ABST
Patent Text Reader

Abstract

The invention provides a carbon dot doped Co3O4 catalyst and a preparation method and application thereof, and relates to the technical field of catalyst preparation, and the preparation method comprises the following steps: mixing a carbon raw material and cobalt salt with an alkaline solution in an organism solution environment, stirring for reaction, filtering and taking precipitate to obtain a solid product; and drying the solid product, and calcining in a protective atmosphere to reduce the size of the carbon raw material and form oxygen vacancies so as to increase the number and activity of active sites and the strength of microwave response, thereby obtaining the carbon dot doped Co3O4 catalyst. The calcining temperature is 300 to 900 DEG C; the carbon dot doped Co3O4 catalyst prepared by the method can effectively increase the active sites of Co3O4, and improve the response of Co3O4 to microwave heating, thereby effectively improving the rate of hydrogen production by hydrolysis of NaBH4.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a carbon dot-doped Co3O4 catalyst and a preparation method and application thereof. Background Art

[0002] Boron hydrides are hydrogen storage materials. By controlling the addition of water and the activity of the catalyst, the rate of hydrogen generation can be effectively controlled. Compared with compressed hydrogen or liquid hydrogen, they are safer to store and transport as solids. Among them, NaBH4 is a common type of borohydride. It has a high hydrogen content and can theoretically reach a hydrogen storage density of 10.8wt%, which makes it an efficient hydrogen storage material. NaBH4 hydrolysis hydrogen production technology is seen as a promising solution for future hydrogen energy applications, especially in the fields of portable energy and transportation. This technology may also be combined with other renewable energy technologies, such as solar energy and wind energy, for efficient energy conversion and storage.

[0003] An efficient catalyst is a key link. This reaction usually requires a catalyst to accelerate the reaction rate. Common catalysts include various metals and their oxides, such as cobalt (Co), nickel (Ni), platinum (Pt), etc. However, these metals and metal oxides are easily deactivated and have high costs. For example, Co3O4 is used as a catalyst for NaBH4 hydrolysis to produce hydrogen, but Co3O4 as a catalyst has the problem of low production efficiency. Microwave enhancement is a technology that uses microwave energy to increase the rate and efficiency of chemical reactions. This method can accelerate the reaction rate in NaBH4 hydrolysis to produce hydrogen technology. However, Co3O4 has a low response to microwaves and cannot effectively increase the reaction rate.

[0004] Therefore, it is necessary to provide a non-metallic catalyst with high catalytic efficiency and strong microwave response. Summary of the invention

[0005] In order to solve the problem of low efficiency of Co3O4 as a catalyst in the prior art in the production of hydrogen by hydrolysis of NaBH4, the present invention provides a carbon dot-doped Co3O4 catalyst and a preparation method and application thereof.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows.

[0007] A method for preparing a carbon dot-doped Co3O4 catalyst comprises the following steps:

[0008] The carbon raw material, the cobalt salt and the organic solvent are mixed and dispersed to obtain a dispersion liquid, and stirred for reaction to obtain a mixed liquid; an alkaline solution is added to the mixed liquid, stirred, and the precipitate is filtered to obtain a solid product;

[0009] After the solid product is dried, it is calcined under a protective atmosphere to reduce the size of the carbon raw material and form oxygen vacancies, so as to increase the number and activity of active sites and the intensity of microwave response, thereby obtaining carbon doped Co3O4;

[0010] The calcination temperature is 300-900°C; if the calcination temperature is lower than 300°C, the formation of Co3O4 will be affected; if the calcination temperature is higher than 900°C, the number of carbon points may decrease, and Co3O4 is also prone to sintering, resulting in an increase in grain size, a decrease in the number of active sites, and a decrease in activity.

[0011] Preferably, the calcination temperature is 300° C., 500° C., 700° C. or 900° C.; the heating rate is 10 to 50° C. / min, and the holding time is 2 to 8 hours.

[0012] The present invention reduces the size of the carbon raw material and forms oxygen vacancies through calcination, wherein the reduction in the size of the carbon raw material can make the activity of the active potential stronger, and the oxygen vacancies can increase the number of active sites, thereby improving the catalytic effect of the carbon doped Co3O4 catalyst. In addition, the presence of oxygen vacancies can lead to enhanced magnetism, and carbon doping can improve electrical conductivity, thereby making it have a better response to microwaves. Moreover, the interface effect between the carbon dots and cobalt oxide can further improve the response intensity to microwaves.

[0013] In another preferred embodiment, the mass ratio of the carbon raw material to the cobalt salt is 1:2 to 8. The present invention improves the effect of carbon doping by controlling the ratio of the carbon raw material to the cobalt salt.

[0014] In another preferred embodiment, the carbon raw material is any one of graphite, carbon nanotubes, graphene, and porous carbon; the cobalt salt is any one of Co(NO3)2, CoCl2, and CoCO3; preferably, the cobalt salt is Co(NO3)2, and the use of Co(NO3)2 as the cobalt salt can improve the purity of the prepared carbon-doped Co3O4 catalyst.

[0015] In another preferred embodiment, the concentration of the alkaline solution is 0.5 to 2 M;

[0016] The alkaline solution is any one of ammonia water, KOH solution, and NaOH solution; the alkaline solution causes Co ions to form Co(OH)2 and precipitate, and then performs subsequent calcination.

[0017] In another preferred embodiment, the alkaline solution is added at a rate of 0.05 to 0.2 ml / s. By controlling the rate of addition, the reaction can be made more uniform; preferably, the alkaline solution is added for no more than 12 minutes.

[0018] In another preferred embodiment, the usage ratio of the cobalt salt to the alkaline solution is 2-8 g:36-72 ml.

[0019] In another preferred embodiment, the usage ratio of the cobalt salt to the organic solution is 2-8 g:100 ml.

[0020] In another preferred embodiment, the organic solvent is any one of anhydrous ethanol, ethylene glycol, methanol, and isopropanol.

[0021] In another preferred embodiment, the drying temperature is 40-80° C., and the drying time is 6-8 hours.

[0022] In another preferred embodiment, during the preparation of the mixed solution, the stirring temperature is room temperature, and the room temperature is 25°C.

[0023] The second invention of the present invention provides a carbon dot-doped Co3O4 catalyst, and the carbon dot-doped Co3O4 catalyst is prepared by the preparation method provided by the first aspect of the present invention.

[0024] The third aspect of the present invention provides a carbon dot-doped Co3O4 catalyst as a catalyst for use in the production of hydrogen by hydrolysis of hydrogen storage materials. The carbon dot-doped Co3O4 catalyst is provided by the second aspect of the present invention. The carbon dot-doped Co3O4 catalyst in the present invention can not only improve the catalytic efficiency of Co3O4, but also has a high response to microwaves, and can further improve the catalytic effect under microwave conditions, thereby effectively increasing the rate of hydrogen production by hydrolysis of borohydrides.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) The present invention can form oxygen vacancies and reduce the size of the carbon raw material after calcination, so that the obtained carbon-doped Co3O4 catalyst has more active sites and the activity of the active sites is improved, thereby effectively improving the rate of hydrogen production by hydrolysis of sodium borohydride. Among them, the presence of oxygen vacancies can lead to enhanced magnetism, and carbon doping can improve electrical conductivity, thereby making the carbon-doped Co3O4 catalyst have a better response to microwaves. In addition, the interface effect between carbon dots and cobalt oxide can further improve the response intensity to microwaves.

[0027] (2) By controlling the ratio of carbon raw materials to cobalt salts, the effect of carbon doping can be effectively improved. Under microwave conditions, the hydrogen production rate of NaBH4 hydrolysis over the prepared carbon dot-doped Co3O4 catalyst reaches 7107 mL / min / g, which is much higher than the hydrogen production rate of 1576 mL / min / g of the Co3O4 catalyst.

[0028] (3) The carbon-doped Co3O4 catalyst prepared by the present invention not only has a high catalytic effect under conventional heating conditions, but also can produce a high response to microwaves under microwave heating conditions, which effectively solves the problem of low microwave response of Co3O4. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 XRD patterns of different catalysts.

[0030] Figure 2 TEM, SAED, HRTEM and EDS images of the carbon-doped Co3O4 catalyst prepared in Example 1 of the present invention; wherein, a) is a TEM image of the Co3O4 catalyst without carbon doping; b) is a TEM image of the carbon dot-doped Co3O4 catalyst, (c) is a TEM image of the carbon dot-doped Co3O4 catalyst after use, (d) and (e) are HRTEM images of the carbon dot-doped Co3O4 catalyst, (f) is a SAED image of the carbon dot-doped Co3O4 catalyst, (g) is a HAADF-STEM image of the carbon dot-doped Co3O4 catalyst, (h) is an EDX image of a mixture of carbon, cobalt and oxygen, (i) is an EDX image of carbon, (j) is an EDX image of cobalt, and (k) is an EDX image of oxygen.

[0031] Figure 3 This is a graph of the hydrogen production rate by hydrolysis of NaBH4 over the carbon-doped Co3O4 catalyst prepared in Examples 1 to 4 of the present invention.

[0032] Figure 4 The rate diagram of hydrogen production by NaBH4 hydrolysis over carbon dot-doped Co3O4 catalysts prepared with different ratios of carbon raw materials to cobalt salts

[0033] Figure 5 This is the hydrogen production rate diagram of NaBH4 hydrolysis over different catalysts.

[0034] Figure 6 This is a graph showing the hydrogen production rate from the hydrolysis of NaBH4 under different conditions. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0036] Unless otherwise specified, the experimental methods described in the following examples are all conventional methods; the reagents and materials described are all commercially available unless otherwise specified.

[0037] NaBH4 hydrolysis hydrogen production technology is seen as a promising solution for future hydrogen energy applications, especially in the field of portable energy and transportation. This technology may also be combined with other renewable energy technologies, such as solar energy and wind energy, for efficient energy conversion and storage. Efficient catalysts are a key link. Currently, non-metallic oxides, such as Co3O4, are used as catalysts for NaBH4 hydrolysis hydrogen production. However, Co3O4 as a catalyst has the problem of low production efficiency.

[0038] Microwave enhancement is a technology that uses microwave energy to increase the rate and efficiency of chemical reactions. This method can accelerate the reaction rate in NaBH4 hydrolysis hydrogen production technology. Microwaves can directly heat the reaction medium and catalyst, so that the active sites of the catalyst reach a temperature suitable for the reaction faster, thereby accelerating the reaction rate of NaBH4 and water. This heating method is more uniform and faster than traditional heating. Through microwave radiation, reaction conditions such as temperature and pressure can be more effectively controlled, which helps to optimize the yield and purity of hydrogen. The use of microwaves can reduce the reaction time, thereby obtaining more hydrogen in a shorter time. Microwaves can also enhance the activity of catalysts by providing additional energy to activate the active sites on the surface of the catalyst. This not only improves the catalytic efficiency, but also reduces the dependence on expensive catalysts (such as platinum) to some extent. In addition, microwave heating is generally more energy-efficient and efficient than traditional heating methods because it directly heats the reactants and catalysts, reducing energy losses. This is an important improvement in the energy efficiency of the entire system. A suitable catalyst that efficiently affects microwaves is essential. However, Co3O4 in the prior art has a low response to microwaves, and thus under microwave heating conditions, Co3O4 cannot effectively increase the rate of hydrogen production.

[0039] The present invention controls the ratio of carbon raw material to cobalt salt to improve the effect of carbon doping, and controls the calcination temperature at 300-900°C by calcination. The calcination temperature below 300°C will affect the formation of Co3O4. The calcination temperature above 900°C may reduce the number of carbon points, and Co3O4 is also easy to sinter, resulting in an increase in grain size, a decrease in the number of active sites, and a decrease in activity. Therefore, the calcination temperature is controlled at 300-900°C to reduce the size of the carbon raw material and form oxygen vacancies, wherein the reduction in the size of the carbon raw material can increase the activity of the active potential, and the oxygen vacancies can increase the number of active sites, thereby improving the catalytic effect of the carbon doped Co3O4 catalyst. In addition, the presence of oxygen vacancies can induce an enhancement of magnetism, and carbon doping can improve electrical conductivity, thereby making it have a better response to microwaves. Moreover, the interface effect between carbon points and cobalt oxide can further improve the response intensity to microwaves. The carbon dot-doped Co3O4 catalyst prepared by the method of the present invention can not only effectively improve the efficiency of hydrogen production by hydrolysis of NaBH4, but also has a high microwave response intensity, thereby further improving the efficiency of hydrogen production by hydrolysis of NaBH4, and effectively solving the problems of low efficiency of hydrogen production by hydrolysis of NaBH4 and poor microwave response of Co3O4 catalyst in the prior art.

[0040] The following is a detailed description of a carbon dot-doped Co3O4 catalyst, its preparation method and its application.

[0041] Example 1

[0042] A method for preparing a carbon dot-doped Co3O4 catalyst comprises the following steps:

[0043] S1. Add graphite and cobalt salt to anhydrous ethanol, and use an ultrasonic cleaning machine to treat them to ensure sufficient dispersion to obtain a dispersion; wherein the cobalt salt is Co(NO3)2; and the amount ratio of graphite, cobalt salt and anhydrous ethanol is 1g:2g:100ml.

[0044] S2. The dispersion was transferred to a reactor, and stirred with a magnetic stirrer at room temperature of 25° C. to obtain a mixed solution.

[0045] S3. Prepare an aqueous ammonia solution with a concentration of 1M and dissolve it in anhydrous ethanol. Use a peristaltic pump to drop the ammonia solution into the reactor containing the mixed solution at a speed of 0.1 ml / s within 10 minutes to allow the reaction to be sufficient and the Co ions to form Co(OH)2 and precipitate. Let the mixed solution stand for 12 hours while continuing to stir at a speed of 300 r / min. Filter the solution after the reaction to obtain the precipitate to obtain a solid product.

[0046] S4. After drying the solid product at 60°C for 6 hours, put it into a tubular furnace and heat it to 300°C in a CO2 atmosphere; wherein the heating rate is set to 10°C / min and maintained at this temperature for 2 hours. After calcination, it is naturally cooled to room temperature in the furnace to obtain a carbon-doped Co3O4 catalyst.

[0047] Example 2

[0048] A method for preparing a carbon dot-doped Co3O4 catalyst comprises the following steps:

[0049] S1. Add carbon nanotubes and cobalt salt into anhydrous ethanol, and use an ultrasonic cleaning machine to treat them to ensure sufficient dispersion to obtain a dispersion; wherein the cobalt salt is Co(NO3)2; and the usage ratio of carbon nanotubes, cobalt salt and anhydrous ethanol is 1g:4g:100ml.

[0050] S2. The dispersion was transferred to a reactor, and stirred with a magnetic stirrer at room temperature of 25° C. to obtain a mixed solution.

[0051] S3. Prepare a 1M NaOH solution and dissolve it in anhydrous ethanol. Use a peristaltic pump to drop the KOH solution into the reactor containing the mixed solution at a rate of 0.1 ml / s over 10 minutes. Let the mixed solution stand for 12 hours while continuing to stir at a rate of 600 r / min. Filter the solution after the reaction to obtain the precipitate to obtain a solid product.

[0052] S4. After drying the solid product at 60°C for 7 hours, put it into a tubular furnace and heat it to 500°C in an air atmosphere; wherein the heating rate is set to 20°C / min and maintained at this temperature for 4 hours. After calcination, it is naturally cooled to room temperature in the furnace to obtain a carbon-doped Co3O4 catalyst.

[0053] Example 3

[0054] A method for preparing a carbon dot-doped Co3O4 catalyst comprises the following steps:

[0055] S1. Add graphene and cobalt salt to anhydrous ethanol, and use an ultrasonic cleaning machine to treat them to ensure sufficient dispersion to obtain a dispersion; wherein the cobalt salt is Co(NO3)2; the amount ratio of graphene, cobalt salt and anhydrous ethanol is 1g:6g:100ml.

[0056] S2. The dispersion was transferred to a reactor, and stirred with a magnetic stirrer at room temperature of 25° C. to obtain a mixed solution.

[0057] S3. Prepare a KOH solution with a concentration of 1 M and dissolve it in anhydrous ethanol. Use a peristaltic pump to drop the NaOH solution into the reactor containing the mixed solution at a speed of 0.1 ml / s within 10 minutes. Let the mixed solution stand for 12 hours while continuing to stir at a stirring speed of 900 r / min. Filter the solution after the reaction to obtain the precipitate to obtain a solid product.

[0058] S4. After drying the solid product at 80°C for 8 hours, put it into a tubular furnace and heat it to 700°C in a nitrogen atmosphere; wherein the heating rate is set to 30°C / min and maintained at this temperature for 6 hours. After calcination, it is naturally cooled to room temperature in the furnace to obtain carbon-doped Co3O4.

[0059] Example 4

[0060] A method for preparing a carbon dot-doped Co3O4 catalyst comprises the following steps:

[0061] S1. Add porous carbon and cobalt salt into anhydrous ethanol, and use an ultrasonic cleaning machine to treat them to ensure sufficient dispersion to obtain a dispersion liquid; wherein the cobalt salt is Co(NO3)2·6H2O; and the usage ratio of porous carbon, cobalt salt and anhydrous ethanol is 1g:8g:100ml.

[0062] S2, transferring the dispersion into a reactor, stirring the mixture with a magnetic stirrer at room temperature of 25° C. to obtain a mixed solution;

[0063] S3, prepare a NaOH solution with a concentration of 1M, and dissolve it in anhydrous ethanol, use a peristaltic pump to drop the NaOH solution into the reactor containing the mixed solution at a speed of 0.1 ml / s within 10 minutes; let the mixed solution stand for 12 hours, continue stirring during this period, and the stirring speed is 1200 r / min, and filter the solution after the reaction to obtain a precipitate to obtain a solid product;

[0064] S4. After drying the filtered solid sample at 80°C for 6 hours, put it into a tubular furnace and heat it to 900°C under an argon atmosphere; wherein the heating rate is set to 50°C / min and maintained at this temperature for 8 hours. After calcination, it is naturally cooled to room temperature in the furnace to obtain a carbon-doped Co3O4 catalyst.

[0065] In order to further illustrate the effect of the carbon dot-doped Co3O4 catalyst prepared by the present invention on the rate of hydrogen production by hydrolysis of NaBH4, we conducted the following experiments.

[0066] 1. Structural characterization of carbon dot-doped Co3O4 catalyst

[0067] Figure 1The XRD diagrams of different catalysts are shown in Figure 1. In the figure, CDs-doped Co3O4 is Co3O4 doped with carbon dots, The spentCDs-doped Co3O4 is Co3O4 doped with carbon dots after use, Pristine Co3O4 is the original Co3O4, Carbon-Co(OH)2 is the intermediate Co(OH)2, and Pristine Carbon is a pure carbon material. Figure 1 It can be seen from the results that the carbon dot-doped Co3O4 crystal form still maintains the crystal form of Co3O4.

[0068] Figure 2 The HRTEM, SAED and EDS images of carbon dot-doped Co3O4 prepared in Example 1, in which CDs represent carbon dots. (a) is the TEM image of the original Co3O4, (b) is the carbon dot-doped Co3O4, and (c) is the carbon dot-doped Co3O4 after use; (d) and (e) are the HRTEM images of carbon dot-doped Co3O4; (f) is the SAED image of carbon dot-doped Co3O4; (g) to (k) are the HAADF-STEM and EDX images of carbon dot-doped Co3O4. Figure 2 It can be seen that carbon dots are doped into Co3O4 material. Figure 2 It can be seen from (g) to (k) that the catalyst in Example 1 contains carbon, cobalt and oxygen, and each element is evenly distributed.

[0069] 2. Catalytic effect of carbon doped Co3O4 catalyst

[0070] Figure 3 The rate diagram of hydrogen production by hydrolysis of NaBH4 at 40°C for the carbon dot-doped Co3O4 catalyst prepared in Examples 1 to 4 of the present invention. Figure 3 It can be seen that the hydrogen production rates of the carbon-doped Co3O4 catalysts prepared in Examples 1 to 4 are all above 4000 mL / min / g, and the hydrogen production rate of Example 3 is the highest.

[0071] The preparation method in Example 1 was adopted, that is, at a calcination temperature of 300°C, the mass ratios of the carbon raw material and the cobalt salt were set to 1:2, 1:4, 1:6, and 1:8, respectively, to obtain carbon dot-doped Co3O4 catalysts with different mass ratios of the carbon raw material and the cobalt salt, and they were used as catalysts in NaBH4 hydrolysis to produce hydrogen, and the hydrogen production rate was recorded. The results are as follows: Figure 4 As shown. Figure 4It can be seen that with the increase of cobalt salt dosage, the hydrogen production rate increases accordingly. When the mass ratio of carbon raw material to cobalt salt is 1:6, the hydrogen production rate reaches a maximum of 7107 mL / min / g. With the increase of cobalt salt content, the hydrogen production rate decreases, but still has a relatively high hydrogen production rate.

[0072] 3. Effect of different catalysts on the rate of hydrogen production by NaBH4 hydrolysis

[0073] Taking the carbon dot-doped Co3O4 catalyst prepared in Example 3 as an example, NaBH4 hydrolysis was carried out to produce hydrogen with pure Co3O4, carbon-doped Co(OH)2, pure Co(OH)2 and pure carbon materials, and the hydrogen production rate was recorded. The results are as follows: Figure 5 shown.

[0074] Figure 5 This is a graph showing the hydrogen production rate of NaBH4 hydrolysis by different catalysts. In the figure, CDs-doped Co3O4 represents carbon-doped Co3O4 catalyst, Pristine Co3O4 represents pure Co3O4, Carbon-Co(OH)2 represents carbon-doped Co(OH)2 catalyst, Pristine Co(OH)2 represents pure Co(OH)2, and Pristine Carbon represents pure carbon material.

[0075] from Figure 5 It can be seen that the hydrogen production rate of Pristine Carbon is as low as 54mL / min / g, the hydrogen production rate of Carbon-Co(OH)2 is 420mL / min / g, the hydrogen production rate of Pristine Co(OH)2 is 1031mL / min / g, and the hydrogen production rate of PristineCo3O4 is 1576mL / min / g. The hydrogen production rate of CDs-doped Co3O4 in the present invention is the highest, reaching 7107mL / min / g. It can be seen that the rate of hydrogen production by hydrolysis of NaBH4 can be effectively improved after calcination and carbon doping. This is mainly due to the fact that the size of the carbon raw material is reduced and oxygen vacancies are formed by calcination, wherein the reduction in the size of the carbon raw material can make the activity of the active potential stronger, and oxygen vacancies can increase the number of active sites, thereby improving the catalytic effect of the carbon doped Co3O4 catalyst.

[0076] 4. Effect of different catalytic conditions on the rate of hydrogen production by hydrolysis of NaBH4

[0077] Figure 6: Comparison of the carbon dot-doped Co3O4 prepared in Example 3 under microwave heating and conventional heating at different temperatures, wherein HGR under conventional heating is the rate of hydrogen production by hydrolysis of NaBH4 by the carbon dot-doped Co3O4 in Example 1 of the present invention under conventional heating, and HGR under MW heating is the rate of hydrogen production by hydrolysis of NaBH4 by the carbon dot-doped Co3O4 in Example 3 of the present invention under microwave. Figure 6 It can be seen that the carbon doped Co3O4 in the present invention can produce hydrogen quickly under both conventional heating and microwave heating, and the hydrogen production rate increases with the increase in temperature. At the same temperature, the rate of hydrogen production under microwave conditions of carbon doped Co3O4 is much higher than the rate of hydrogen production under conventional heating, and as the temperature increases, the growth rate of hydrogen production under microwave conditions is faster than the growth rate of hydrogen production under conventional heating. This is mainly due to the fact that the size of the microwave response is related to magnetism and conductivity. The greater the magnetism and the stronger the conductivity, the better the response to microwaves. In the carbon doped Co3O4 catalyst in Example 3 of the present invention, the presence of oxygen vacancies can induce an enhancement of magnetism, and carbon doping can improve conductivity, thereby making it have a better response to microwaves. In addition, the interface effect between carbon dots and cobalt oxide can further improve the intensity of the response to microwaves.

[0078] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a carbon dot-doped Co3O4 catalyst, characterized in that: The following steps are involved: The carbon raw material and the cobalt salt are mixed with the alkaline solution in an organic solvent environment, stirred for reaction, and the precipitate is filtered to obtain a solid product; After the solid product is dried, it is calcined under a protective atmosphere to reduce the size of the carbon raw material and form oxygen vacancies, thereby increasing the number and activity of active sites and the intensity of microwave response, thereby obtaining a carbon-doped Co3O4 catalyst; The calcination temperature is 300-900°C.

2. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The mass ratio of the carbon raw material to the cobalt salt is 1:2-8.

3. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The carbon raw material is any one of graphite, carbon nanotubes, graphene, and porous carbon; the cobalt salt is any one of Co(NO3)2, CoCl2, and CoCO3.

4. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The concentration of the alkaline solution is 0.5 to 2 M; The alkaline solution is any one of ammonia water, KOH solution and NaOH solution.

5. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The dropping speed of the alkaline solution is 0.05-0.2 ml / s.

6. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The usage ratio of the cobalt salt to the alkaline solution is 2-8 g:36-72 ml.

7. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The usage ratio of the cobalt salt to the organic solution is 2-8 g:100 ml.

8. The method for preparing a carbon dot-doped Co3O4 catalyst according to claim 1, characterized in that: The organic solvent is any one of anhydrous ethanol, ethylene glycol, methanol and isopropanol.

9. A carbon-doped Co3O4 catalyst prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the carbon-doped Co3O4 catalyst according to claim 9 as a catalyst in the production of hydrogen by hydrolysis of hydrogen storage materials.