Design and preparation of novel catalyst for reaction of preparing propylene by dehydrogenation of COpropane oxide

By using a bimetallic Pt-Co/CeOx@SiO2 catalyst in the CO2 oxidation propane dehydrogenation reaction, the strong electrostatic adsorption method is used to improve the dispersion and anti-sintering ability of the active metal, solving the stability and environmental friendliness of the traditional Pt-based catalyst. problem, achieving efficient propane conversion and CO2 utilization.

CN118807775APending Publication Date: 2024-10-22NINGXIA UNIVERSITY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410788777.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Traditional Pt-based catalysts have problems such as short life, low stability, high cost, and easy carbon deposition in the CO2 oxidation propane dehydrogenation reaction. Moreover, Cr-based catalysts are toxic and difficult to improve activity and stability in an environmentally friendly manner.

Method used

A new bimetallic Pt-Co/CeOx@SiO2 catalyst is designed and synthesized. CeOx nanoclusters are synthesized on SiO2 as a carrier through strong electrostatic adsorption method to improve the dispersion of active metals and through the introduction of Co under high temperature reaction conditions. Enhance the sintering resistance and stability of the catalyst.

Benefits of technology

It achieves high propane conversion rate, CO2 conversion rate and propylene selectivity, extends the service life of the catalyst, has a simple preparation method, is environmentally friendly, and has excellent regeneration performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807775A_ABST
    Figure CN118807775A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalyst preparation, and particularly provides a preparation method of a novel catalyst for propylene preparation reaction (CO2-OPDH) through CO2 propane oxide dehydrogenation. The method comprises the following steps: (1) firstly, synthesizing CeOx nanoclusters with the mass fraction of 25% on gas-phase SiO2 by adopting a strong electrostatic adsorption method, and drying and roasting to obtain a carrier CeOx coated SiO2 of the catalyst; (2) dropwise adding a certain amount of a mixed solution of chloroplatinic acid and cobalt nitrate into the carrier while stirring in an ultrasonic state; and (3) drying and roasting the uniformly stirred initial wet mixture to obtain the catalyst. The prepared catalyst is used for CO2-OPDH reaction, the preparation method is simple, environment-friendly and excellent in regeneration performance, and the catalyst can have high propane conversion rate, CO2 conversion rate and propylene selectivity at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and particularly relates to a novel catalyst for CO2 oxidation propane dehydrogenation to propylene reaction and a preparation method thereof. Background Art

[0002] As a major emerging propylene production technology, propane direct dehydrogenation (PDH) technology has effectively alleviated the over-reliance on petroleum resources to produce propylene, but it has problems such as high reaction temperature, low propylene selectivity and easy carbon deposition. The CO2 oxidation propane dehydrogenation (CO2-OPDH) route to propylene can not only reduce reaction energy consumption, but also effectively utilize CO2 and reduce carbon emissions, becoming one of the research hotspots in recent years. At present, the catalysts used in the PDH process are mainly Pt-based and Cr-based catalysts. However, Cr-based catalysts are toxic and easy to pollute the environment, so their use is limited. Although Pt-based catalysts have problems such as short life, low stability and high cost, they have attracted much attention because they have strong activation ability for propane CH bonds and are not easy to activate CC bonds, and are environmentally friendly. The main reason for the deactivation of Pt-based catalysts is the presence of carbon deposition and the sintering of Pt nanoparticles, so it is necessary to improve the activity and stability of Pt-based catalysts. Adding additives can not only improve the dispersion of Pt, but also help improve the anti-sintering ability and stability of the catalyst, and extend the service life of the catalyst.

[0003] In view of the problems existing in traditional Pt-based catalysts and from the perspective of environmental friendliness and economic benefits, finding a suitable second metal to modify them is an attractive strategy. As a non-precious metal propane dehydrogenation catalyst, Co-based catalyst has great application potential in PDH due to its abundant resources, low price, low toxicity and strong activation ability for alkane CH bonds. Although the introduction of a second metal has great potential in improving the activity of the catalyst and inhibiting the formation of carbon deposits, under high temperature reaction conditions, the bimetallic active components still have problems such as easy agglomeration of metal particles, uneven dispersion and poor stability.

[0004] Since the properties of the carrier will also directly affect the catalytic activity and stability of Pt-based catalysts, modifying the commonly used carriers or designing new carriers will help to improve the dispersion of active metals on the carrier surface and reduce its grain size, thereby improving the performance of the catalyst. Li et al. prepared a new functional nano-colloid carrier CeO by strong electrostatic adsorption. x @SiO2, CeO x The nanoclusters act as functional nanoglue to position Pt atoms for CO oxidation. x The nanoclusters are adsorbed on the SiO2 with a large specific surface area through strong electrostatic interaction to form a highly dispersed island structure.x It can anchor metal atoms and improve the dispersion of active metals. The abundant oxygen vacancies on its surface can optimize the adsorption energy of reactants on the catalyst surface, thereby reducing the reaction energy barrier, promoting molecular activation, and making it easier to interact with the stable C=O in CO2. In addition, the oxygen vacancies in the catalyst can synergize with nearby active metal sites. Therefore, it is a good strategy to use the unique advantages of this support structure as a support for catalysts in the CO2-OPDH reaction. Summary of the invention

[0005] Based on the above analysis of the advantages of active metals, additives and carriers, and targeting the problems of traditional Pt-based catalysts, the present invention designed and synthesized a new bimetallic Pt-Co / CeO x @SiO2 catalyst is used in CO2-OPDH reaction. It is not only simple to prepare, environmentally friendly, and has excellent regeneration performance, but also has the advantages of high propane conversion rate, CO2 conversion rate, and propylene selectivity.

[0006] The present invention provides a method for preparing a novel catalyst for the reaction of CO2 oxidation of propane to produce propylene by dehydrogenation, and the specific process is achieved by the following steps:

[0007] (1) First, a strong electrostatic adsorption method was used to synthesize 25% CeO on the gas phase SiO2. x Nanoclusters, this process requires strict control of the pH value of the solution, after filtration, drying and calcination, the catalyst carrier CeO x @SiO2;

[0008] (2) Mixing the precursor solutions containing the platinum source and the cobalt source respectively according to the mass percentage to obtain a solution 1, and then slowly immersing the solution 1 in the CeO x @SiO2 carrier, stirring while ultrasonicating;

[0009] (3) The uniformly stirred initial wet mixture is subjected to ultrasonic treatment, drying, calcination, reduction and other steps to obtain a catalyst product.

[0010] In the step (1), the gas phase SiO2 is hydrophilic and has a specific surface area ranging from 250 to 450 m 2 / g, and the cerium source is selected from cerium nitrate hexahydrate.

[0011] In the step (1), CeO x @The calcination temperature of the SiO2 carrier is 500-600°C, preferably 500°C, and the calcination time is 12h. The drying temperature is 80-120°C, preferably 80°C, and the drying time is 12h.

[0012] In the step (1), the pH value of the solution needs to be controlled at about 8.7.

[0013] In the step (2), the types of platinum source and cobalt source are not limited, wherein the platinum source is selected from one of chloroplatinic acid hexahydrate, chloroplatinic acid and platinum tetrachloride, preferably chloroplatinic acid. The cobalt source is selected from one of cobalt nitrate hexahydrate and cobalt chloride, preferably cobalt nitrate hexahydrate.

[0014] In the step (2), the solvent used for the precursor solution of the platinum source and the cobalt source is selected from deionized water, ethanol, and methanol, preferably deionized water.

[0015] In the step (2), the contents of Pt and Co are expressed in mass percentage, wherein the Pt content is fixed at 0.5%, and the Co content is 0.5-1.5%.

[0016] In the step (3), the ultrasonic time is 30 minutes, the drying temperature is 80-120°C, preferably 80°C, and the drying time is 12 hours. The roasting temperature is 500-600°C, preferably 550°C, and the roasting time is 4 hours. The reduction temperature is 500-600°C, preferably 500°C, and the reduction time is 2 hours.

[0017] The supported bimetallic Pt-Co / CeO prepared by the present invention x @The application of SiO2 system catalyst in the CO2 oxidation propane dehydrogenation to propylene reaction, the specific reaction conditions are as follows:

[0018] (1) The catalyst was heated in an Ar atmosphere from room temperature at 5°C min -1 The temperature was raised to 500°C, and then the reducing gas was switched to H2 / N2=5 / 95, and the reduction was carried out at 500-600°C under normal pressure for 2h, preferably at 500°C. The gas flow rate was 20mL·min -1 Then, the temperature was increased from 500°C to 5°C min in an Ar atmosphere. -1 The temperature was raised to the reaction temperature and then switched to raw gas C3H8 / CO2 / Ar=1:1:8.

[0019] (2) The reaction was carried out in a fixed bed reactor under normal pressure, with a feed gas flow rate of 10 to 30 mL min -1 , preferably 20 mL·min -1 .

[0020] (3) The amount of the catalyst used is 0.1-0.2 g, preferably 0.15 g. The reaction temperature of the catalyst is 500-600° C., preferably 550° C., and the reaction time is 5 h.

[0021] The supported bimetallic Pt-Co / CeO prepared by the present invention x@SiO2 catalyst has the following advantages:

[0022] (1) Prepared bimetallic Pt-Co / CeO x @The preparation method of SiO2 catalyst is simple, environmentally friendly and has excellent regeneration performance.

[0023] (2) CeO prepared by strong electrostatic adsorption method x @SiO2 carrier has a unique structure, among which CeO x The nanoclusters act as nano-glue, and the abundant oxygen vacancies on their surface are not only beneficial for activating CO2 and propane, but also for anchoring active metals and improving the dispersion of active metals. The introduction of Co further promotes the dispersion of Pt. The close contact between the Pt-Co bimetallics and the interaction between electrons significantly improve the reaction activity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 XRD spectra of catalyst-4 prepared in Example 4 of the present invention and catalyst-6 prepared in Comparative Example 1;

[0025] Figure 2 The activity data diagram of the catalysts prepared in Examples 1 to 5 of the present invention and Comparative Example 1;

[0026] Figure 3 This is a data graph showing the activity of Catalyst-4 prepared in Example 4 of the present invention changing with time. DETAILED DESCRIPTION

[0027] Embodiment 1:

[0028] Firstly, a strong electrostatic adsorption method was used to synthesize 25% CeO on SiO2. x The nanoclusters were prepared in the following steps: 1.08 g of fumed SiO2 powder was mixed with 300 mL of deionized water, and the resulting aqueous solution was subjected to ultrasonic treatment to produce a uniform mixture. Under vigorous stirring, 0.93 g of Ce(NO3)3·6H2O was dissolved in the above solution, and a certain amount of NH3·H2O was quickly injected. The stirring was continued for 3 min. The pH value of the final solution was about 8.7. The precipitate was collected by vacuum filtration and air-dried at room temperature overnight. The dried powder was ground and then calcined at 500°C in a muffle furnace for 12 h to obtain CeO x @SiO2 carrier. Then take 1g CeO x @SiO2, add an appropriate amount of chloroplatinic acid solution while stirring with the assistance of ultrasound. After ultrasound for 30 minutes, put it in an oven and dry it at 80°C for 12 hours. Finally, place the dried catalyst in a muffle furnace and calcine it at 550°C for 4 hours to obtain catalyst-1, in which the mass fraction of Pt is 0.5%.

[0029] Embodiment 2:

[0030] Firstly, a strong electrostatic adsorption method was used to synthesize 25% CeO on SiO2. x The nanoclusters were prepared in the following steps: 1.08 g of fumed SiO2 powder was mixed with 300 mL of deionized water, and the resulting aqueous solution was subjected to ultrasonic treatment to produce a uniform mixture. Under vigorous stirring, 0.93 g of Ce(NO3)3·6H2O was dissolved in the above solution, and a certain amount of NH3·H2O was quickly injected. The stirring was continued for 3 min. The pH value of the final solution was about 8.7. The precipitate was collected by vacuum filtration and air-dried at room temperature overnight. The dried powder was ground and then calcined at 500°C in a muffle furnace for 12 h to obtain CeO x @SiO2 carrier. Then take 1g CeO x @SiO2, add an appropriate amount of cobalt nitrate hexahydrate solution while stirring with the assistance of ultrasound. After ultrasound for 30 minutes, put it in an oven and dry it at 80°C for 12 hours. Finally, place the dried catalyst in a muffle furnace and calcine it at 550°C for 4 hours to obtain catalyst-2, in which the mass fraction of Co is 1.0%.

[0031] Embodiment 3:

[0032] Firstly, a strong electrostatic adsorption method was used to synthesize 25% CeO on SiO2. x The nanoclusters were prepared in the following steps: 1.08 g of fumed SiO2 powder was mixed with 300 mL of deionized water, and the resulting aqueous solution was subjected to ultrasonic treatment to produce a uniform mixture. Under vigorous stirring, 0.93 g of Ce(NO3)3·6H2O was dissolved in the above solution, and a certain amount of NH3·H2O was quickly injected. The stirring was continued for 3 min. The pH value of the final solution was about 8.7. The precipitate was collected by vacuum filtration and air-dried at room temperature overnight. The dried powder was ground and then calcined at 500°C in a muffle furnace for 12 h to obtain CeO x @SiO2 carrier. Then take 1g CeO x @SiO2, add an appropriate amount of chloroplatinic acid and cobalt nitrate hexahydrate mixed solution while stirring with the assistance of ultrasound. After ultrasound for 30 minutes, put it in an oven and dry it at 80°C for 12 hours. Finally, place the dried catalyst in a muffle furnace and calcine it at 550°C for 4 hours to obtain catalyst-3, in which the mass fraction of Pt is 0.5% and the mass fraction of Co is 0.5%.

[0033] Example 4

[0034] Firstly, a strong electrostatic adsorption method was used to synthesize 25% CeO on SiO2. xThe nanoclusters were prepared in the following steps: 1.08 g of fumed SiO2 powder was mixed with 300 mL of deionized water, and the resulting aqueous solution was subjected to ultrasonic treatment to produce a uniform mixture. Under vigorous stirring, 0.93 g of Ce(NO3)3·6H2O was dissolved in the above solution, and a certain amount of NH3·H2O was quickly injected. The stirring was continued for 3 min. The pH value of the final solution was about 8.7. The precipitate was collected by vacuum filtration and air-dried at room temperature overnight. The dried powder was ground and then calcined at 500°C in a muffle furnace for 12 h to obtain CeO x @SiO2 carrier. Then take 1g CeO x @SiO2, add an appropriate amount of chloroplatinic acid and cobalt nitrate hexahydrate mixed solution while stirring with the assistance of ultrasound. After ultrasound for 30 minutes, put it in an oven and dry it at 80°C for 12 hours. Finally, place the dried catalyst in a muffle furnace and calcine it at 550°C for 4 hours to obtain catalyst-4, in which the mass fraction of Pt is 0.5% and the mass fraction of Co is 1.0%.

[0035] The inventors used X-ray diffractometer to characterize the crystal structure of catalyst-4 in Example 4. The results are as follows: Figure 1 As shown in the figure, the catalyst exhibits a cubic fluorite crystal structure. Compared with the crystal structure of catalyst-6 prepared in comparative example 1, it has a strong and broad characteristic diffraction peak, and the diffraction peak is slightly shifted to a lower angle compared to the (111) crystal plane of CeO2, indicating that CeO x @SiO2 forms a unique structure different from CeO2 crystals. In addition, no characteristic diffraction peaks of Pt or Co were observed in the samples loaded with active metals, indicating that the active components in the prepared catalyst are highly dispersed on the surface of the molecular sieve. This may also be due to the fact that the Pt and Co contents are too low, exceeding the minimum detection limit of the instrument.

[0036] Example 5

[0037] Firstly, a strong electrostatic adsorption method was used to synthesize 25% CeO on SiO2. x The nanoclusters were prepared in the following steps: 1.08 g of fumed SiO2 powder was mixed with 300 mL of deionized water, and the resulting aqueous solution was subjected to ultrasonic treatment to produce a uniform mixture. Under vigorous stirring, 0.93 g of Ce(NO3)3·6H2O was dissolved in the above solution, and a certain amount of NH3·H2O was quickly injected. The stirring was continued for 3 min. The pH value of the final solution was about 8.7. The precipitate was collected by vacuum filtration and air-dried at room temperature overnight. The dried powder was ground and then calcined at 500°C in a muffle furnace for 12 h to obtain CeO x @SiO2 carrier. Then take 1g CeO x@SiO2, add an appropriate amount of chloroplatinic acid and cobalt nitrate hexahydrate mixed solution while stirring with the assistance of ultrasound. After ultrasound for 30 minutes, put it in an oven and dry it at 80°C for 12 hours. Finally, place the dried catalyst in a muffle furnace and calcine it at 550°C for 4 hours to obtain catalyst-5, in which the mass fraction of Pt is 0.5% and the mass fraction of Co is 1.5%.

[0038] Comparative Example 1

[0039] First, CeO2 and SiO2 with a mass fraction of 25% were fully ground by physical mixed grinding, and then calcined at 550°C in a muffle furnace for 4 hours to obtain a CeO2&SiO2 carrier. Then, 1g of CeO2&SiO2 was taken, and an appropriate amount of chloroplatinic acid and cobalt nitrate hexahydrate mixed solution was added dropwise while stirring under the assistance of ultrasound. After ultrasound for 30 minutes, it was placed in an oven and dried at 80°C for 12 hours. Finally, the dried catalyst was placed in a muffle furnace and calcined at 550°C for 4 hours to obtain Catalyst-6, in which the mass fraction of Pt was 0.5% and the mass fraction of Co was 1.0%.

[0040] Example 6

[0041] 0.15 g of the catalyst-1 prepared in Example 1 and 0.15 g of quartz sand were mixed evenly and loaded into a fixed bed reactor. Then, the reactor was heated from room temperature at 5 °C min-1 under an Ar atmosphere. -1 The temperature was raised to 500°C, and the reducing gas was switched to H2 / N2 = 5 / 95. The reduction was carried out at 500°C and atmospheric pressure for 2 h. The gas flow rate was 20 mL min -1 Then, the temperature was increased from 500°C to 5°C min in an Ar atmosphere. -1 The temperature was raised to 550°C, and then the raw gas was switched to C3H8 / CO2 / Ar = 1:1:8. The reaction was carried out at 550°C and normal pressure. The raw gas flow rate was 20 mL min -1 , the air velocity is about 8000mL / (g cat h), the activity results are as follows Figure 2 The initial conversion of propane was 13.7%, the initial conversion of CO2 was 81.2%, and the initial selectivity of propylene was 65.6%.

[0042] Example 7

[0043] The catalytic activity of catalyst-2 in Example 2 in the CO2 oxidation propane dehydrogenation reaction to produce propylene was determined using the method of Example 6. The initial conversion of propane was 2.9%, the initial conversion of CO2 was 19.3%, and the initial selectivity of propylene was 54.9%. The activity results are shown in Figure 6. Figure 2 shown.

[0044] Example 8

[0045] The catalytic activity of catalyst-3 in Example 3 in the CO2 oxidation propane dehydrogenation to propylene reaction was determined using the method of Example 6. The initial conversion of propane was 23.3%, the initial conversion of CO2 was 67.3%, and the initial selectivity of propylene was 82.1%. The activity results are shown in Figure 6. Figure 2 shown.

[0046] Example 9

[0047] The catalytic activity of catalyst-4 in Example 4 in the CO2 oxidation propane dehydrogenation to propylene reaction was determined by the method of Example 6. The initial conversion of propane was 30.6%, the initial conversion of CO2 was 61.6%, and the initial selectivity of propylene was 86.0%. The activity results are shown in FIG. Figure 2 shown. Figure 3 This is a graph showing the change in catalytic activity of catalyst-4 over reaction time. As can be seen from the graph, the conversion rate of propane gradually decreases over time, but the selectivity of propylene is very high and stable.

[0048] Example 10

[0049] The catalytic activity of catalyst-5 in Example 5 in the CO2 oxidation propane dehydrogenation to propylene reaction was determined by the method of Example 6. The initial conversion of propane was 23.5%, the initial conversion of CO2 was 65.8%, and the initial selectivity of propylene was 85.6%. The activity results are shown in FIG. Figure 2 shown.

[0050] Embodiment 11

[0051] The catalytic activity of catalyst-6 in comparative example 1 in the CO2 oxidation propane dehydrogenation to propylene reaction was determined by the method of Example 6. The initial conversion rate of propane was 3.6%, the initial conversion rate of CO2 was 19.9%, and the initial selectivity of propylene was 61.9%. The activity results are shown in FIG. Figure 2 shown.

[0052] The embodiments described above are detailed descriptions of the technical solutions of the present invention, which should be understood as specific implementation measures of the present invention and are not used to summarize the present invention. Any modifications, supplements or similar replacements made within the scope of the principles of the present invention shall fall within the scope of protection that the present invention should enjoy.

Claims

1. A method for preparing a novel catalyst for the reaction of CO2 oxidation of propane to propylene, characterized in that This is accomplished by following these steps: (1) First, a strong electrostatic adsorption method was used to synthesize 25% CeO on the gas phase SiO2. x Nanoclusters, this process requires strict control of the pH value of the solution, after filtration, drying and calcination, the catalyst carrier CeO x @SiO2; (2) Mixing the precursor solutions containing the platinum source and the cobalt source respectively according to the mass percentage to obtain a solution 1, and then slowly immersing the solution 1 in the CeO x @SiO2 carrier, stirring while ultrasonicating; (3) The uniformly stirred initial wet mixture is subjected to ultrasonic treatment, drying, calcination, reduction and other steps to obtain a catalyst product.

2. The method for preparing the catalyst according to claim 1, characterized in that: The gas phase SiO2 in step (1) is hydrophilic and has a specific surface area ranging from 250 to 450 m 2 / g, and the cerium source is mainly selected from cerium nitrate hexahydrate.

3. The method for preparing the catalyst according to claim 1, characterized in that: The calcination temperature in step (1) is 500-600° C., the calcination time is 12 hours, the drying temperature is 80-120° C., and the drying time is 12 hours.

4. The method for preparing the catalyst according to claim 1, characterized in that: The types of the platinum source and the cobalt source in step (2) are not limited, wherein the platinum source is selected from one of chloroplatinic acid hexahydrate, chloroplatinic acid and platinum tetrachloride, and the cobalt source is selected from one of cobalt nitrate hexahydrate and cobalt chloride.

5. The method for preparing the catalyst according to claim 1, characterized in that: The contents of Pt and Co in step (2) are expressed in mass percentage, wherein the mass fraction of Pt is fixed at 0.5%, and the mass fraction of Co is 0.5-1.5%.

6. The method for preparing the catalyst according to claim 1, characterized in that: In step (3), the ultrasonic time is 30 minutes, the drying temperature is 80-120° C., and the drying time is 12 hours.

7. The method for preparing the catalyst according to claim 1, characterized in that: In step (3), the calcination temperature is 550-600° C., the calcination time is 4 hours, the reduction temperature is 500-600° C., and the reduction time is 2 hours.

8. The supported bimetallic Pt-Co / CeO was prepared according to the preparation method and conditions described in claims 1 to 7. x @SiO2 system catalyst.

9. A supported bimetallic Pt-Co / CeO as claimed in claim 8 x @The application of SiO2 system catalyst in the CO2 oxidation propane dehydrogenation to propylene reaction is characterized by The specific reaction conditions are as follows: (1) The catalyst was heated in an Ar atmosphere from room temperature at 5°C min -1 The temperature was raised to 500°C, and then the reducing gas was switched to H2 / N2 = 5 / 95, and the reduction was carried out at 500-600°C under normal pressure for 2 h. The gas flow rate was 20 mL min -1 Then, the temperature was kept at 5℃·min in Ar atmosphere. -1 The temperature was raised to the reaction temperature, and then the raw gas was switched to C3H8 / CO2 / Ar=1:1:8; (2) The reaction was carried out in a fixed bed reactor under normal pressure, with a feed gas flow rate of 10 to 30 mL min -1 ; (3) The amount of the catalyst used is 0.1-0.2 g, the reaction temperature of the catalyst is 500-600° C., and the reaction time is 5 h.

Citation Information

Patent Citations

  • Catalyst for preparing propylene through propane oxidation and preparation method and application thereof

    CN112473659A

  • Reaction catalyst for preparing propylene by oxidizing propane with CO2

    CN114345343A

  • PtSn catalyst with supported modified carrier, preparation method of PtSn catalyst and application of PtSn catalyst in propane dehydrogenation coupling reverse water gas

    CN116943647A

  • Oxidative dehydrogenation catalyst

    WO2022249616A1