Silver-based catalyst for ethylene epoxidation and preparation method thereof

Through the synergy of high-energy ball milling and additives, a silver-based catalyst with high selectivity and less waste liquid is prepared, which solves the problems of low catalyst selectivity and large waste liquid in the existing technology, and improves the efficiency of ethylene oxide production.

CN118807779APending Publication Date: 2024-10-22NINGBO JINYUANDONG PETROCHEM ENG TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410958420.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing ethylene epoxidation catalysts have low selectivity, produce a large amount of waste liquid during the preparation process, and have a high loading of precious metals, which affects the efficiency of ethylene oxide production.

Method used

A high-energy ball milling method is used to mix the silver precursor with an alumina carrier, and by adding copper and cobalt compounds as additives, high-energy ball milling and roasting are performed to prepare a silver-based catalyst, which reduces the generation of waste liquid and improves the selectivity of the catalyst.

Benefits of technology

The selectivity and activity of the catalyst are improved, the precious metal loading is reduced, the preparation process is simplified, the generation of waste liquid is reduced, and the process is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807779A_ABST
    Figure CN118807779A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a silver-based catalyst for ethylene epoxidation. The preparation method comprises the following steps: (1) uniformly mixing a silver precursor and an alumina carrier to obtain a mixed material; (2) putting the mixed material into a grinding tank, simultaneously putting grinding balls and a solvent into the grinding tank, grinding for a certain time through a high-energy ball mill, adding an auxiliary agent precursor, continuously grinding, and obtaining a mixed viscous material after the grinding is completed; and (3) drying the viscous material, and roasting in an air or nitrogen atmosphere by using a tubular furnace to prepare the silver-based catalyst. The catalyst disclosed by the invention is prepared by using a high-energy ball milling method, and the compound of metal Ag and auxiliaries Cu and Co is loaded on the alumina carrier, so that the preparation method is simple, less waste liquid is generated, and the interaction between the metal Ag and the carrier and between the metal Ag and the auxiliaries Cu and Co and the dispersion uniformity of metal elements are improved; therefore, the catalyst has high activity and selectivity in the ethylene epoxidation reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ethylene epoxidation catalysts, and in particular to a silver-based catalyst for ethylene epoxidation and a preparation method thereof. Background Art The ethylene oxide catalyst currently used in industry is Ag / Al2O3, while Cs, Re, etc. are used as chemical or structural additives to improve the catalyst activity or selectivity. The main preparation method is the impregnation method, and the catalyst selectivity is about 85%.

[0003] Patent CN201810621828.7 discloses a silver impregnation solution and a silver catalyst for producing ethylene oxide by epoxidation of ethylene, and a preparation method thereof. The silver impregnation solution for producing ethylene oxide by epoxidation of ethylene contains the following components: 1) a silver-ammine complex; 2) a polar amino acid; 3) water; 4) an optional auxiliary agent; wherein the content of the polar amino acid is 0.05 to 60 wt % based on the total weight of the impregnation solution. The catalyst preparation method disclosed in the patent is an impregnation method, and a large amount of waste liquid is generated during the preparation process. The selectivity of the catalyst is lower than 85%, and its selectivity needs to be further improved in actual industrial applications.

[0004] In addition, in order to save the cost of preparing the catalyst and improve the efficiency of ethylene oxide production, effectively reducing the silver loading and changing the content or composition of the metal additive is an effective method. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a silver-based catalyst for ethylene epoxidation and a preparation method thereof. The catalyst obtained by the method has high selectivity, low precious metal loading, and reduces the generation of waste liquid.

[0006] The present invention solves the above technical problems through the following technical solutions: A method for preparing a silver-based catalyst for ethylene epoxidation comprises the following steps: (1) uniformly mixing a silver precursor and an alumina carrier to obtain a mixed material; (2) putting the above-mentioned mixed material into a grinding jar, and putting grinding balls and solvent into the grinding jar at the same time, grinding for a certain period of time with a high-energy ball mill, and then adding the auxiliary agent precursor to continue grinding, and obtaining a mixed viscous material after the grinding is completed; (3) The viscous material is dried and then calcined in an air or nitrogen atmosphere using a tubular furnace to prepare a silver-based catalyst.

[0007] Further, based on the mass of metal Ag, the metal Ag is 2-20% of the mass of the alumina support, preferably 5-15%.

[0008] Furthermore, the silver precursor is selected from at least one of silver oxalate, silver oxide and silver nitrate.

[0009] Further, the auxiliary agent precursor includes a copper compound and a cobalt compound; Preferably, the copper compound and the cobalt compound are selected from nitrates or oxalates.

[0010] Furthermore, based on the mass of metallic Ag, the mass ratio of metallic copper to metallic Ag in the copper compound is 0.03-0.3:1; the mass ratio of metallic cobalt to metallic Ag in the cobalt compound is 0.03-0.3:1.

[0011] Furthermore, during ball milling, the diameters of the grinding balls are 20 mm, 15 mm, 10 mm, 7 mm and 5 mm, respectively, and the number ratio of the grinding balls with diameters of 20 mm, 15 mm, 10 mm, 7 mm and 5 mm is 1:2:8:10:60; The rotation speed during ball milling is 100-500 r / min, and the total ball milling time is 4-6 h.

[0012] Furthermore, the volume ratio of the mixture to the solvent in step (2) is 1:(0.5-3); Preferably, the volume ratio of the mixture to the solvent is 1:1.5.

[0013] Further, the solvent is at least one of ethyl acetate and isopropanol, preferably ethyl acetate; Preferably, the solvent contains pyrophosphoric acid.

[0014] Furthermore, in step (3), the viscous material is first dried in an oven and then calcined in a tubular furnace under the following calcination conditions: heating at 1-10°C / min and calcining at 150-650°C for 30-360 minutes; Preferably, the calcination conditions are: heating at 2-5°C / min, and calcination at 250-450°C for 120-240 minutes.

[0015] A silver-based catalyst for ethylene epoxidation is obtained according to any one of the above preparation methods.

[0016] Compared with the prior art, the present invention has the following advantages: 1. The present invention provides a silver-based catalyst for ethylene epoxidation, which is prepared by a high-energy ball milling method. The high-energy ball milling method has a strong force during its preparation process, can improve the interaction between the metal and the carrier, and is helpful for better loading of the metal elements onto the carrier, thereby improving the activity of the catalyst; in addition, by first loading the silver compound for a certain period of time and then loading the auxiliary compound, the synergistic effect between the metal Ag and the auxiliary agents Cu and Co is enhanced, so that the catalyst has a higher selectivity.

[0017] 2. The silver-based catalyst for ethylene epoxidation provided by the present invention adds a specific amount of solvent during the ball milling process, which can better dissipate heat, prevent overheating and degradation of the grinding material, and also help to evenly disperse the particles, making the catalyst performance more consistent. At the same time, it can make the metal more easily dispersed and anchored on the carrier, improve the dispersion, and then improve the catalyst activity.

[0018] 3. The silver-based catalyst for ethylene epoxidation provided by the present invention uses cheap Cu and Co compounds, has fewer operating steps, a simple preparation process, less waste liquid, and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A schematic diagram of a reaction device for detecting catalyst activity and selectivity according to the present invention; Figure 2 XRD spectra of the catalysts prepared in Examples 1-3 of the present invention; Figure 3 This is a SEM image of the α-Al2O3 carrier without metal oxide loading in the present invention; Figure 4 This is a SEM image of catalyst 1 prepared in Example 1 of the present invention; Figure 5 This is a SEM image of catalyst 2 prepared in Example 2 of the present invention; Figure 6 This is a SEM image of catalyst 3 prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] The basic concept of the technical solution of the present invention is as follows: A method for preparing a silver-based catalyst for ethylene epoxidation comprises the following steps: (1) Stir and mix appropriate amounts of silver precursor and α-Al2O3 carrier to obtain a mixed material.

[0022] Calculated by the mass of metal Ag, the metal Ag accounts for 2-20% of the mass of the alumina support, preferably 5-15%.

[0023] (2) The mixture obtained in step (1) is placed in an 80 ml hardened stainless steel grinding jar (planetary high energy ball mill PM300, Retsch), and an appropriate amount of solvent (ethyl acetate or isopropanol) is added. At the same time, 5, 10, 40, 100, and 300 grinding balls with diameters of 20 mm, 15 mm, 10 mm, 7 mm, and 5 mm are placed in the grinding jar, respectively. The ball milling speed is 100 to 500 r / min. After grinding for a certain period of time, the additives of copper and cobalt compounds are added. The total ball milling time is 4 to 6 hours.

[0024] Calculated by the mass of metallic Ag, the mass ratio of metallic copper to metallic Ag in the copper compound is 0.03-0.3:1; similarly, the mass ratio of metallic cobalt to metallic Ag in the cobalt compound is 0.03-0.3:1.

[0025] After the ball milling is completed, the grinding balls are taken out to obtain the sticky material in the grinding jar.

[0026] (3) Dry the viscous material obtained in step (2) in an oven at 105° C. for 12 hours. Then, use a tubular furnace in an air or nitrogen atmosphere with a gas flow rate of 100-300 mL / min and a heating rate of 1-10° C. / min to calcine at 150-650° C. for 30-360 minutes to prepare a catalyst.

[0027] Specifically, the silver precursor is selected from at least one of silver oxalate, silver oxide and silver nitrate; and the copper compound and the cobalt compound are selected from nitrate or oxalate. Specifically, the volume ratio of the mixture to the solvent is 1:(0.5-3); preferably, the volume ratio of the mixture to the solvent is 1:1.5. Specifically, the solvent contains pyrophosphoric acid, and the volume of the pyrophosphoric acid is 0.05-0.2 times the volume of the solvent.

[0028] Example 1 (1) Weigh 20 g of α-Al2O3 carrier (with a diameter less than 4 mm) and place it in an 80 ml hardened stainless steel ball mill (planetary high energy ball mill PM300, Retsch), then add 5.5 g of silver nitrate into the grinding jar and mix evenly to obtain a mixed material.

[0029] (2) Ethyl acetate is added to the mixed material obtained in step (1), wherein the volume of ethyl acetate is 1.5 times the volume of the mixed material, wherein ethyl acetate contains pyrophosphoric acid, and the volume of pyrophosphoric acid is 0.1 times the volume of ethyl acetate. At the same time, 5, 10, 40, 100, and 300 grinding balls with diameters of 20 mm, 15 mm, 10 mm, 7 mm, and 5 mm, respectively, are placed in a grinding jar, the ball milling speed is 300 r / min, and the ball milling time is 2 h.

[0030] Then, 0.97 g Cu(NO3)2·3H2O and 1.24 g Co(NO3)2·6H2O were placed into the above ball mill and the grinding was continued for 3 h.

[0031] After the ball milling is completed, the grinding balls are taken out, and the grinding balls are washed with ethyl acetate to obtain a filtrate, and the filtrate is filtered to obtain a filter cake, and the filter cake is mixed with the remaining material in the grinding tank to obtain a viscous material.

[0032] (3) The viscous material obtained in step (2) was dried in an oven at 105° C. for 12 hours, and then calcined at 350° C. for 240 minutes in a tubular furnace under air atmosphere with a gas flow rate of 300 mL / min and a heating rate of 2° C. / min to prepare catalyst 1.

[0033] Example 2 Compared with Example 1, the amount of silver nitrate added was 3.5 g, and other conditions were the same as those of Example 1. The prepared catalyst was named Catalyst 2.

[0034] Example 3 Compared with Example 2, the masses of Cu(NO3)2·3H2O and Co(NO3)2·6H2O are 0.31 g and 0.87 g respectively, and other conditions are the same as those of Example 2. The prepared catalyst is named Catalyst 3.

[0035] X-ray diffraction phase analysis (XRD) The metal oxide crystal phase testing instrument was a D / MAX2500 X-ray diffractometer (Rigaku, Japan), and a Cu Kα target, graphite monochromator and nickel filter were selected to detect the specific content of different metals in the catalyst.

[0036] Test conditions: 200mA tube current, 40KV tube voltage, emission and scattering are set to 1°, set the receiving parameters to 1.5×104m, 0.02° step width, and finally use the external standard α-SiO2 for the correction angle value. Determination method: First, grind the experimental sample into powder and press it into a piece to meet the test requirements, then gently insert it into the sample stage of the goniometer, and set the program to record the spectrum and scan continuously. The XRD spectra of the specific α-Al2O3 carrier and the catalyst prepared in Examples 1-3 are as follows Figure 2 As shown (where Figure 2 Catalyst 1 represents the XRD spectrum of catalyst 1 prepared in Example 1, and the peaks corresponding to the black dots in the figure are the characteristic peaks of metal Ag; Catalyst 2 represents the XRD spectrum of catalyst 2 prepared in Example 2; Catalyst 3 represents the XRD spectrum of catalyst 3 prepared in Example 3; Support represents the XRD spectrum of α-Al2O3 support).

[0037] The chemical composition was analyzed using a Rigaku ZSX Primus II X-ray fluorescence spectrometer. A rhodium (Rh) target was selected as the anode target, and five spectroscopic crystals were used. The equipment is also equipped with a scintillation detector and a gas flow proportional detector; the optical path operates under vacuum conditions, and the Ar and CH4 mixed gases on the instrument are used as detector gases. The collimator mask in the instrument has a specification of Φ27mm, and adopts a maximum output power of 3kW and a maximum output voltage of 60kV. A YYJ-40 semi-automatic sample press was used for sample preparation. The mass fractions of different metals in the catalysts of the above Examples 1-3 are summarized in Table 1 below.

[0038] Table 1 catalyst Ag content (wt%) Cu content (wt%) Co content (wt%) Catalyst 1 14.8 1.0 1.1 Catalyst 2 10.3 0.9 1.0 Catalyst 3 10.2 0.3 0.7 Example 4 Compared with Example 1, the silver precursor is silver oxalate, the amount of silver oxalate added is 3.2 g, and other conditions are the same as those of Example 2. The prepared catalyst is named Catalyst 4.

[0039] Example 5 Compared with Example 1, the amount of silver nitrate added was 4.72 g, the masses of Cu(NO3)2·3H2O and Co(NO3)2·6H2O were 1.13 g and 4.37 g respectively, and the other conditions were the same as those of Example 1. The prepared catalyst was named Catalyst 5.

[0040] Example 6 Compared with Example 1, the amount of silver nitrate added is 0.63 g, and the masses of Cu(NO3)2·3H2O and Co(NO3)2·6H2O are 0.05 g and 0.58 g respectively; the solvent added in step (2) is isopropanol, the volume of which is 3 times the volume of the mixed material, and pyrophosphoric acid is added to the isopropanol, the volume of which is 0.05 times the volume of the isopropanol.

[0041] After the ball milling was completed, the grinding balls were taken out and washed with isopropanol to obtain a filtrate. Other conditions were the same as those in Example 1. The prepared catalyst was named Catalyst 6.

[0042] The contents of the various metal components in the catalyst preparation process of the above-mentioned Examples 1-6 are summarized in Table 2 below.

[0043] Table 2 Comparative Example 1 Compared with Example 1, only Cu(NO3)2·3H2O was added, and Co(NO3)2·6H2O was not added. Other conditions were the same as those in Example 1. The prepared catalyst was named Comparative Sample 1.

[0044] Comparative Example 2 Compared with Example 1, only Co(NO3)2·6H2O was added, and Cu(NO3)2·3H2O was not added. Other conditions were the same as those in Example 1. The prepared catalyst was named Comparative Sample 2.

[0045] Comparative Example 3 Compared with Example 1, pyrophosphoric acid was not added to ethyl acetate in step (2), and other conditions were the same as those in Example 1. The prepared catalyst was named Comparative Sample 3.

[0046] Comparative Example 4 Compared with Example 1, in step (2), 0.97 g Cu(NO3)2·3H2O and 1.24 g Co(NO3)2·6H2O were mixed with silver nitrate and the carrier in step (1) to obtain a mixed material, the grinding time in step (2) was 5 h, and the other conditions were the same as those in Example 1. The prepared catalyst was named Comparative Sample 4.

[0047] Catalyst activity and selectivity detection methods The catalysts of Examples 1-5 and Comparative Examples 1-4 were first tableted and sieved to obtain catalyst particles of 40-60 mesh, and then a performance evaluation experiment was conducted using a laboratory micro fixed bed reactor. The specific method is: A stainless steel reaction tube with an inner diameter of 10 mm is placed in a three-stage heating furnace. The constant temperature section is ensured to be 7-10 cm, the catalyst loading is 4 ml, and the loading items of the reaction tube are glass wool, 40-60 mesh quartz sand, 40-60 mesh catalyst particles, and 40-60 mesh quartz sand from bottom to top. When loading, ensure that the catalyst is in the middle of the reaction heating furnace.

[0048] The reaction conditions are as follows: The contents of ethylene, oxygen and nitrogen in the reaction gas were 28 mol%, 7 mol% and 65 mol% respectively, of which nitrogen contained 5 ppm of ethyl chloride, the reaction temperature was 230°C, the reaction pressure was 2 MPa, and the space velocity was 5200 h -1 The reaction results were analyzed using an Agilent 7820 chromatograph, in which the FID detector was used to detect ethylene and ethylene oxide, and the TCD detector was used to detect nitrogen, oxygen and carbon dioxide. The specific double reactor reaction device for preparing ethylene oxide by epoxidation of ethylene is as follows: Figure 1 shown.

[0049] The specific results of the catalyst activity and selectivity tested are shown in Table 3 below.

[0050] Table 3 Ethylene conversion rate (%) Ethylene oxide selectivity (%) Catalyst 1 11.7 93.6 Catalyst 2 10.2 95.3 Catalyst 3 8.5 95.0 Catalyst 4 8.9 94.2 Catalyst 5 9.1 94.2 Comparison sample 1 8.0 79.6 Comparison sample 2 8.6 80.7 Comparison sample 3 6.9 83.5 Comparison sample 4 7.9 81.5 From the catalyst activity and selectivity results in Table 2 above, it can be seen that in the process of preparing the catalyst, if no metal compound of copper or cobalt is added, the ethylene oxide selectivity of the catalyst will be significantly affected in the end; in addition, in the process of ball milling, adding pyrophosphoric acid to the solvent can also improve the catalyst activity for ethylene epoxidation reaction and the selectivity for ethylene oxide.

[0051] In addition, during the catalyst preparation process, when the silver compound, the copper compound and the cobalt compound are ground simultaneously, it is found that the activity and selectivity of the finally prepared catalyst are reduced.

[0052] Scanning electron microscopy (SEM) Hitachi S-4800 scanning electron microscope was used to observe the morphology, particle size and other information of the catalyst sample. Determination method: The catalyst sample was pre-sprayed with gold, the conductive glue was evenly covered on the sample holder, and then different areas were selected for observation and imaging. The specific SEM image of the α-Al2O3 carrier without metal oxide loading is shown in Figure 3 As shown; the SEM image of catalyst 1 prepared in Example 1 is as shown Figure 4 As shown; the SEM image of catalyst 2 prepared in Example 2 is as shown Figure 5 As shown; the SEM image of catalyst 3 prepared in Example 3 is as shown Figure 6 shown.

[0053] Comparative Example 5 The solvent added in step (2) is ethanol, and the other conditions are the same as those in Example 1. The catalyst prepared is named Comparative Sample 5.

[0054] Comparative Example 6 In step (2), 10, 40 and 100 grinding balls with diameters of 15 mm, 10 mm and 7 mm, respectively, are placed in a grinding jar, the ball milling speed is 300 r / min, and the ball milling time remains unchanged.

[0055] The other conditions were the same as those in Example 1, and the prepared catalyst was named Comparative Sample 6.

[0056] Comparative Example 7 The calcination conditions in step (3) are a heating rate of 15°C / min and calcination at 650°C for 7h.

[0057] The other conditions were the same as those in Example 1, and the prepared catalyst was named Comparative Sample 7.

[0058] Specific surface area analysis The specific surface area and pore distribution of the sample were tested by mercury intrusion method, which is to press mercury into the pore structure under precisely controlled pressure to measure the specific surface area and pore distribution, etc. The instrument used is the V9610 mercury intrusion instrument produced by the American Micromeritics Company. Determination method: The sample is first fully dried at 110-120℃, and then low-pressure analysis and high-pressure analysis are carried out in turn to obtain the specific surface data of the silver catalyst.

[0059] The specific surface area parameters of the catalysts prepared in Specific Example 1 and Comparative Examples 5-7 and the corresponding ethylene conversion rates are shown in Table 4 below.

[0060] Table 4 <![CDATA[Specific surface area (m 2 / g)]]> Ethylene conversion rate (%) Catalyst 1 9.1 11.7 Comparison sample 5 8.5 6.6 Comparison sample 6 8.7 4.9 Comparison sample 7 8.9 5.9 It can be seen from the specific surface area results in Table 3 above that different solvents added during the ball milling process or changes in the diameter and number of the selected grinding balls, as well as changes in the calcination conditions during the catalyst preparation process, will affect the activity of the catalyst.

Claims

1. A method for preparing a silver-based catalyst for ethylene epoxidation, characterized in that: The steps include: (1) uniformly mixing a silver precursor and an alumina carrier to obtain a mixed material; (2) Put the above mixed material into a grinding jar, put grinding balls and solvent into the grinding jar, grind it for a certain period of time with a high-energy ball mill, add the auxiliary agent precursor and continue grinding, and obtain a mixed viscous material after grinding; (3) The viscous material is dried and then calcined in a tubular furnace under air or nitrogen atmosphere to prepare a silver-based catalyst.

2. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 1, characterized in that: Calculated by the mass of metallic Ag, the metallic Ag accounts for 2-20% of the mass of the alumina support, preferably 5-15%.

3. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 1, characterized in that: The silver precursor is selected from at least one of silver oxalate, silver oxide and silver nitrate.

4. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 1, characterized in that: The auxiliary agent precursor includes a copper compound and a cobalt compound; Preferably, the copper compound and the cobalt compound are selected from nitrates or oxalates.

5. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 4, characterized in that: Calculated by the mass of metallic Ag, the mass ratio of metallic copper to metallic Ag in the copper compound is 0.03-0.3:1; the mass ratio of metallic cobalt to metallic Ag in the cobalt compound is 0.03-0.3:

1.

6. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 1, characterized in that: During ball milling, the diameters of the grinding balls are 20 mm, 15 mm, 10 mm, 7 mm and 5 mm, respectively, and the number ratio of the grinding balls with diameters of 20 mm, 15 mm, 10 mm, 7 mm and 5 mm is 1:2:8:20:60; The rotation speed during ball milling is 100-500 r / min, and the total ball milling time is 4-6 h.

7. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 1, characterized in that: The volume ratio of the mixed material to the solvent in step (2) is 1:(0.5-3); Preferably, the volume ratio of the mixture to the solvent is 1:1.

5.

8. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 7, characterized in that: The solvent is at least one of ethyl acetate and isopropanol, preferably ethyl acetate; Preferably, the solvent contains pyrophosphoric acid.

9. The method for preparing a silver-based catalyst for ethylene epoxidation according to claim 1, characterized in that: In step (3), the viscous material is first dried in an oven and then calcined in a tubular furnace under the following calcination conditions: heating at 1-10°C / min and calcining at 150-650°C for 30-360 minutes; Preferably, the calcination conditions are: heating at 2-5°C / min, and calcination at 250-450°C for 120-240 minutes.

10. A silver-based catalyst for ethylene epoxidation, characterized in that Obtained according to the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Carrier of silver catalyst for producing epoxy ethane, preparation method and application of carrier of silver catalyst

    CN102145285A

  • Preparation method of precious metal-supported alpha-Al2O3 powder catalysis material

    CN107362796A

  • Silver catalyst for ethylene epoxidation reaction, and preparation method and application thereof

    CN111013585A

  • Preparation method and application of mesoporous aluminum oxide supported noble metal rhodium dehydrogenation catalyst

    CN113198467A

  • Alpha-alumina carrier, preparation method thereof, silver catalyst and application

    CN117181207A