Catalyst for preparing high-carbon alcohol from synthesis gas as well as preparation method and application of catalyst
By using small-sized, multi-scale porous molybdenum sulfide materials in the synthesis gas to high-carbon alcohol reaction, the problem of low sulfur vacancy active sites and insufficient pore structure at the edge of the MoS2-based catalyst is solved, and high activity and high selectivity catalytic effects are achieved. , suitable for industrial applications.
Patent Information
- Application Number
- CN202310393268.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-22
AI Technical Summary
In the reaction of synthesis gas to high-carbon alcohols, the existing MoS2-based catalysts have large nanosheet sizes, low edge sulfur vacancy active site concentration, and lack of multi-scale pore structure, resulting in low catalytic activity and selectivity, and the diffusion of reactant and product molecules. difficulty.
Using small-sized, multi-scale porous molybdenum sulfide materials, array-arranged molybdenum sulfide nanosheets are formed through the interaction between templates and precursors. They have abundant edge sulfur vacancies and multi-scale pore structures to achieve full contact between reactants and active sites. and rapid detachment of products, and regulate the pore structure to improve catalytic activity and selectivity.
It significantly improves the catalyst activity and high-carbon alcohol selectivity, has high carbon monoxide conversion rate and stability, and is suitable for industrial applications.
Smart Images

Figure BDA0004176623080000111 
Figure BDA0004176623080000112 
Figure BDA0004176623080000121
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst for preparing higher alcohols from synthesis gas and a preparation method and application thereof, and belongs to the field of chemistry and chemical engineering. Background Art
[0002] Higher carbon alcohols are generally C 2+ Alcohols can be used as solvents, chemical raw materials, alternative fuels and fuel additives. The increasing scarcity of petroleum resources makes it of great strategic significance to develop new non-oil-based carbon resource conversion routes to synthesize carbon-containing chemicals or fuels. Among them, converting non-oil-based carbon resources such as coal, natural gas, biomass and even CO2 into high-carbon alcohols via synthesis gas (mainly a mixture of CO and H2, containing a small amount of CO2) is an extremely attractive path.
[0003] At present, for the reaction of synthesizing high-carbon alcohols from synthesis gas, researchers have developed several catalyst systems including modified Rh-based catalysts, Mo-based catalysts, modified methanol synthesis catalysts and modified Fischer-Tropsch synthesis catalysts. Among them, molybdenum sulfide (MoS2)-based catalysts have attracted widespread attention due to their relatively low price and unique sulfur resistance. After a lot of optimization, the overall selectivity of synthesizing gas to alcohols catalyzed by molybdenum sulfide-based catalysts has been able to reach a high level, but methanol is still usually the main alcohol product, and its selectivity often accounts for more than 50% of the total alcohols, which greatly limits the application prospects of molybdenum sulfide-based catalysts. People usually improve the activity and C of molybdenum sulfide-based catalysts by adding a second transition metal (such as Fe, Co, Ni, Rh, etc.). 2+ Although the reaction is selective for alcohol, the formation of a large amount of hydrocarbon by-products is often difficult to avoid, and the reaction process often faces the loss of the second transition metal component caused by the formation of carbonyl compounds or the deactivation caused by the sintering of the second transition metal.
[0004] The production of high-carbon alcohols from syngas involves the breaking of CO bonds and the coupling of CC bonds, and the edge sulfur vacancy active sites of MoS2-based catalysts are crucial to the above two key steps, directly affecting the activity and selectivity of the reaction. However, most of the MoS2-based syngas-to-high-carbon alcohol catalysts reported so far use H2S as the sulfur source, and simply load MoS2 on carbon or oxide carriers. The synthesized MoS2 nanosheets are large in size and have low concentrations of edge sulfur vacancy active sites. They also lack multi-scale pore structures, making it difficult for reactant and product molecules to diffuse, and therefore face problems such as low activity and low selectivity. Designing a new structure of molybdenum sulfide-based catalysts to increase the concentration of edge sulfur vacancy active sites and the molecular diffusion rate in the pores, thereby obtaining high activity and high alcohol selectivity, is of great significance for the industrial application of syngas-to-high-carbon alcohols. Summary of the invention
[0005] The purpose of the present invention is to provide a catalyst for preparing high-carbon alcohols from synthesis gas, and its preparation method and application. The present invention uses small-sized, multi-scale porous molybdenum sulfide materials for preparing high-carbon alcohols from synthesis gas for the first time, significantly reducing the size of molybdenum sulfide nanosheets, increasing the concentration of active sites of edge sulfur vacancies, and realizing the controllable construction of multi-scale porous structures of molybdenum sulfide materials, promoting the diffusion of molecules in the pores, thereby breaking through the key technical bottlenecks such as low active site concentration of molybdenum sulfide catalyst systems and slow diffusion of reactant and product molecules. In addition, the small-sized, multi-scale porous molybdenum sulfide catalyst disclosed in the present invention has a self-supporting effect and does not require any carrier assistance. The catalyst exhibits the characteristics of high carbon monoxide conversion rate, high selectivity for high-carbon alcohols, good stability, etc., and has good industrial application prospects and commercial value.
[0006] The present invention discloses a method for preparing a catalyst for preparing high-carbon alcohols from synthesis gas, wherein a small-sized, multi-scale porous molybdenum sulfide material is grown on a suitable template, and after being modified with an alkali metal, it is used for preparing high-carbon alcohols from synthesis gas. The molybdenum sulfide synthesized by the method is arranged in an array and presents a small lateral size, so it has abundant edge sulfur vacancies, making it highly active. In addition, the method disclosed in the present invention can enable the synthesized molybdenum sulfide material to completely replicate the template structure, and by adjusting the properties of the template itself and its interaction with the precursor, the pore structure of the synthesized molybdenum sulfide material can be regulated. Through the catalyst preparation method disclosed in the present invention, the controllable construction of multi-scale porous molybdenum sulfide materials with one-dimensional linear pores, two-dimensional linear cross pores or three-dimensional spherical pores and their composite pore structures can be achieved. The synthesized molybdenum sulfide catalyst has a multi-scale pore structure, which promotes the diffusion of reactant and product molecules, so that the reactant molecules can fully contact the active sites; and enables the product molecules to quickly leave the catalyst bed, inhibiting the occurrence of secondary side reactions, and significantly improving the catalytic activity and selectivity.
[0007] The invention is described in detail as follows:
[0008] A catalyst for preparing high-carbon alcohols from synthesis gas, characterized in that the catalyst for preparing high-carbon alcohols from synthesis gas is a small-sized, multi-scale porous molybdenum sulfide material modified with an alkali metal, which has abundant sulfur vacancies at the edge of the molybdenum sulfide; the porous pore skeleton of the porous molybdenum sulfide material is formed by the molybdenum sulfide itself; and it does not contain a carrier or a template agent.
[0009] The size of the molybdenum sulfide nanosheets in the above materials is 0.5 to 15 nm, which belongs to small-sized molybdenum sulfide;
[0010] The multi-scale porous structure is composed of micropores (0.2-2 nm) between molybdenum sulfide nanosheets and mesopores, macropores or both formed by the support of the molybdenum sulfide nanosheet skeleton, and the inner diameter of the pores is 2-400 nm; the mesopores or macropores are at least one of one-dimensional linear pores, two-dimensional linear cross pores or three-dimensional spherical pores; the preferred average pore size of the mesopores or macropores is 6-400 nm.
[0011] A preparation method of a catalyst for preparing high-carbon alcohols from synthesis gas can be summarized as follows: by selecting a suitable template A, a molybdenum source B is uniformly dispersed on the template A or a surface-treated template A*, and then a sulfur source C is introduced, and the molybdenum source B and the sulfur source C are reacted in situ at high temperature to obtain a reaction product D in one step, and then the reaction product D is transferred to a post-treatment liquid E for treatment to wash away the template, and a small-sized, multi-scale porous molybdenum sulfide material F is obtained by suction filtration and washing, and the molybdenum sulfide material F is uniformly mixed with an alkali metal additive G to obtain a catalyst H for preparing high-carbon alcohols from synthesis gas;
[0012] The template A is at least one of silica spheres, silica nanowires, SBA-15, KIT-6, alumina nanowires, titanium oxide nanowires, titanium oxide nanospheres, and titanium oxide nanotubes, and the diameters of the above-mentioned oxide spheres, oxide nanowires, and oxide nanotubes are 2 to 400 nm; the molybdenum source B is at least one of ammonium molybdate, sodium molybdate, potassium molybdate, phosphomolybdic acid, sodium phosphomolybdate, potassium phosphomolybdate, molybdenum chloride, and molybdenum acetylacetonate; the sulfur source C is thiourea, sulfur, sodium sulfide, potassium sulfide, hydrogen sulfide, ammonium tetrathiomolybdate, carbon disulfide, dimethyl sulfoxide, At least one of thioacetamide, cysteine, methionine, and mercaptan; the molar ratio of molybdenum atoms to sulfur atoms in the molybdenum source B and the sulfur source C is 1:1 to 1:500; the post-treatment liquid E is at least one of hydrofluoric acid solution, sulfuric acid solution, hydrochloric acid solution, nitric acid solution, sodium hydroxide solution, potassium hydroxide solution, and ammonia solution; the alkali metal additive G is at least one of lithium, sodium, potassium, and cesium hydroxide or metal salt compounds, preferably potassium carbonate or potassium hydroxide; the molar ratio of the alkali metal additive G to the alkali metal atom to the molybdenum atom in molybdenum sulfide is 0.02 to 5;
[0013] The method for obtaining the template A* by surface treatment is at least one of hydroxylation, amination, carboxylation and alkylation;
[0014] The method for uniformly dispersing the molybdenum source B on the template A or the surface-treated template A* is at least one of ultrasonic dispersion, mixed grinding, and ball milling.
[0015] 1) The ultrasonic frequency is 10 to 300 kHz. The specific steps of the ultrasonic dispersion method are: (1) first add the template A or A* into a dispersant and ultrasonically disperse for 0.5 to 6 hours. The dispersant is water, methanol, ethanol, propanol, acetone, or a mixed solution thereof; the concentration of the template and the dispersant to form a dispersion is 1 g / L to 1000 g / L; (2) add the molybdenum source B into the above dispersion and ultrasonically disperse for 0.5 to 6 hours;
[0016] 2) The specific steps of the mixed grinding method are: mixing the template A or A* and the molybdenum source B in a mortar, and mixing and grinding for 0.5 to 6 hours;
[0017] 3) The specific steps of the ball milling method are: mixing the template A or A* and the molybdenum source B in a ball milling jar, placing the ball milling jar on a ball mill for 2 to 50 hours. The material of the ball milling jar is at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and hard alloy; the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, or hard alloy balls; the ball-to-material ratio is 200:1 to 10:1 (mass ratio); the ball milling speed is 200 to 1500 rpm.
[0018] The molybdenum sulfide material F and the alkali metal additive G are mixed by at least one of a liquid phase dispersion stirring method, a mixed grinding method, and a ball milling method:
[0019] 1) The specific steps of the liquid phase dispersion and stirring method are: (1) dissolving the alkali metal additive G in a solvent to form a solution, wherein the solvent is at least one of water, methanol, ethanol, acetone, and N,N-dimethylformamide (DMF); (2) adding the molybdenum sulfide material F to the above solution and ultrasonically dispersing it for 0.5 to 6 hours to form a dispersion; (3) placing the above dispersion at 25 to 150° C. and stirring it until dry, thereby achieving uniform mixing of the molybdenum sulfide material F and the alkali metal additive G; the ultrasonic frequency is 10 to 300 kHz.
[0020] 2) The specific steps of the mixed grinding method are: mixing the molybdenum sulfide material F and the alkali metal additive G in a mortar, and mixing and grinding for 0.5 to 6 hours;
[0021] 3) The specific steps of the ball milling method are: mixing the molybdenum sulfide material F and the alkali metal additive G in a ball milling jar, placing the ball milling jar on a ball mill for 2 to 50 hours. The material of the ball milling jar is at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and hard alloy; the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, or hard alloy balls; the ball-to-material ratio is 200:1 to 10:1 (mass ratio); the ball milling speed is 200 to 1500 rpm.
[0022] The catalyst is used for preparing high-carbon alcohols from synthesis gas and is suitable for one or more of a fixed bed reactor, a fluidized bed reactor, a moving bed reactor, a slurry bed reactor and a kettle reactor.
[0023] Before the catalyst is used in the synthesis gas to produce high carbon alcohol reaction, it is pretreated at 180-600°C for 0.5-50 hours in an inert atmosphere, a reducing atmosphere or a mixed atmosphere of the two, which, on the one hand, increases the concentration of sulfur vacancy active sites, and on the other hand, allows the alkali metal promoter to diffuse rapidly on the catalyst surface and more evenly react with the sulfur vacancy active sites. The inert atmosphere is at least one of nitrogen, argon, helium, and neon; the reducing atmosphere is at least one of hydrogen, carbon monoxide, and hydrogen sulfide; the synthesis gas atmosphere is at least one of CO / H2 and CO / CO2 / H2; and the high carbon alcohol is at least one of alcohols containing more than 2 carbon atoms.
[0024] Compared with the prior art, the beneficial effects of the synthesis gas to higher alcohol catalyst and its preparation method and application provided by the present invention are mainly reflected in the following aspects:
[0025] (1) Aiming at the problem that the conventional MoS2-based syngas-to-high alcohol catalyst nanosheets are large in size and have a low concentration of edge sulfur vacancy active sites, the present invention utilizes the strong interaction between the template and the precursor to arrange the synthesized molybdenum sulfide in an array, completely replicate the template structure, and present a smaller lateral size, thereby having abundant edge sulfur vacancy active sites.
[0026] (2) The conventional MoS2-based catalyst for synthesizing high-carbon alcohols from synthesis gas lacks a multi-scale pore structure, and the reactant and product molecules have difficulty in diffusing. The present invention adjusts the properties of the template itself and its interaction with the precursor to control the pore structure of the synthesized molybdenum sulfide material, thereby achieving the controllable construction of a multi-scale porous molybdenum sulfide material having one-dimensional linear pores, two-dimensional linear cross pores or three-dimensional spherical pores and their composite pore structures. The constructed multi-scale pore structure can promote the diffusion of reactant and product molecules, allowing the reactant molecules to fully contact the active sites; and enable the product molecules to quickly leave the catalyst bed, thereby inhibiting the occurrence of secondary side reactions and significantly improving the catalytic activity and selectivity.
[0027] (3) This invention is the first to use small-sized, multi-scale porous molybdenum sulfide materials for the production of higher alcohols from syngas, breaking through key technical bottlenecks such as low active site concentration and slow diffusion of reactant and product molecules in the molybdenum sulfide catalyst system. The catalyst exhibits high carbon monoxide conversion rate, high selectivity for higher alcohols, and good stability, and has good industrial application prospects and commercial value. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 1 to 11 are TEM images of catalysts MoS2-1 to 11 in the examples and comparative examples, respectively;
[0029] According to the size statistics of molybdenum sulfide nanosheets, the sizes of MoS2-1-4 and MoS2-8-10 are all less than 10nm; while the sizes of MoS2-5-7 and MoS2-11 are all greater than 20nm, even greater than 200nm. The TEM images, XRD images and corresponding catalytic properties have been analyzed in detail in the examples and comparative examples;
[0030] Figure 2 In are the XRD spectra of the catalysts MoS2-1 to 11 in the examples and comparative examples respectively;
[0031] Figure 3 The following are the O2 adsorption infrared spectra of the catalysts MoS2-2 and MoS2-7 in the embodiment and the comparative example, wherein 900-980cm -1 The wave number is the characteristic peak of O2 adsorption by sulfur vacancies at the edge of MoS2, 800 cm -1 The wide packet nearby is the characteristic peak of O2 adsorption by in-plane sulfur vacancies. The results show that MoS2-2 has abundant edge sulfur vacancies. DETAILED DESCRIPTION
[0032] The following examples illustrate the catalyst for preparing higher alcohols from synthesis gas provided by the present invention, and its preparation method and application, but the present invention is not limited thereto.
[0033] Regarding the mixing method of the template and the precursor, such as non-specific template, the ultrasonic dispersion method, the mixed grinding method and the ball milling method achieve similar effects, so the following embodiments and comparative examples all take ultrasonic dispersion as an example.
[0034] Example 1
[0035] 1200mg of ammonium molybdate and 5333mg of silica sphere dispersion (ethylene glycol dispersion containing 30wt% silica, silica sphere diameter of about 100-200nm) were uniformly dispersed in 100mL of deionized water, ultrasonically dispersed for 6 hours, the ultrasonic frequency was 120kHz, then stirred dry at room temperature, and then vacuum dried in a vacuum drying oven at 120℃. The dried sample was packaged in a 100mL stainless steel autoclave with 20mL of carbon disulfide under argon protection and reacted at 450℃ for 6 hours. The obtained product was treated in a potassium hydroxide solution at 80℃ for 24 hours to remove the silica template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80℃. It is recorded as MoS2-1.
[0036] According to XRD characterization, MoS2-1 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed, and the MoS2-1 catalyst does not contain a carrier or a template agent. According to TEM characterization, MoS2-1 completely replicates the silica sphere template, and the MoS2 nanosheets are stacked to form a three-dimensional macroporous skeleton with an inner diameter of about 150nm; in addition, the MoS2 nanosheets are stacked to form micropores (stacked pores), and this multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 6.2nm. The small size of MoS2 nanosheets gives it abundant edge sulfur vacancies, thus showing high activity and high selectivity.
[0037] Example 2
[0038] 1600 mg of ammonium molybdate tetrahydrate and 2500 mg of SBA-15 (pore inner diameter of about 6-13 nm) were uniformly dispersed in 100 mL of deionized water, ultrasonically dispersed for 12 hours at an ultrasonic frequency of 120 kHz, then stirred to dry at room temperature, and then dried in an oven at 80 ° C overnight. The dried sample was packaged in a 100 mL stainless steel autoclave with 40 mL of carbon disulfide under argon protection and reacted at 500 ° C for 12 hours. The product was treated in a hydrofluoric acid solution at room temperature for 8 hours to remove the SBA-15 template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80 ° C. It is recorded as MoS2-2.
[0039] According to XRD characterization, MoS2-2 is a typical 2H-MoS2 structure, and there is no XRD signal of silicon dioxide, indicating that the template has been completely removed, and the MoS2-2 catalyst does not contain a carrier or a template agent. According to TEM characterization, MoS2-2 completely replicates the SBA-15 template, and the MoS2 nanosheets are orderly arranged along the original spatial structure of SBA-15 to form a one-dimensional linear structure, forming a mesoporous skeleton with an inner diameter of about 10nm; in addition, the MoS2 nanosheets form micropores (stacked pores) by stacking, and this multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 3.6nm. The small size of MoS2 nanosheets makes it have abundant edge sulfur vacancies, thus showing high activity and high selectivity.
[0040] Example 3
[0041] 1200 mg of ammonium molybdate tetrahydrate and 2500 mg of SiO2 microspheres (diameter about 400 nm) were uniformly dispersed in 100 mL of deionized water, ultrasonically dispersed for 6 hours at an ultrasonic frequency of 120 kHz, then stirred to dry at room temperature, and then dried in an oven at 120 ° C overnight. The dried sample was packaged in a 100 mL stainless steel autoclave with 20 mL of carbon disulfide under argon protection and reacted at 450 ° C for 6 hours. The obtained product was treated in a potassium hydroxide solution at 80 ° C for 24 hours to remove the SiO2 template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80 ° C. Recorded as MoS2-3.
[0042] According to XRD characterization, MoS2-3 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed, and the MoS2-3 catalyst does not contain a carrier or a template agent. According to TEM characterization, MoS2-3 completely replicates the silica microsphere template, and the MoS2 nanosheets are stacked to form a three-dimensional macroporous skeleton with an inner diameter of about 400nm; in addition, the MoS2 nanosheets are stacked to form micropores (stacked pores), and this multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 5.5nm. The small size of MoS2 nanosheets gives it abundant edge sulfur vacancies, thus showing high activity and high selectivity.
[0043] Example 4
[0044] 1200 mg of ammonium molybdate tetrahydrate and 2500 mg of aminated SiO2 microspheres (diameter about 400 nm) were uniformly dispersed in 100 mL of deionized water, ultrasonically dispersed for 6 hours at an ultrasonic frequency of 120 kHz, then stirred to dry at room temperature, and then dried in an oven at 120 ° C overnight. The dried sample was packaged in a 100 mL stainless steel autoclave with 20 mL of carbon disulfide under argon protection and reacted at 450 ° C for 6 hours. The product was treated in a potassium hydroxide solution at 80 ° C for 24 hours in a hydrofluoric acid solution to remove the SiO2 template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80 ° C. It is recorded as MoS2-4.
[0045] According to XRD characterization, MoS2-4 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed, and the MoS2-4 catalyst does not contain a carrier or a template agent. According to TEM characterization, MoS2-4 completely replicates the silica microsphere template, and the MoS2 nanosheets are stacked to form a three-dimensional macroporous skeleton with an inner diameter of about 400nm; in addition, the MoS2 nanosheets form micropores (stacked pores) through stacking. This multi-scale pore structure is conducive to the mass transfer of reactants, products and intermediate molecules. Due to the amino treatment, the interaction between the molybdenum precursor and the surface of the silica sphere template is enhanced, avoiding polymerization during the high-temperature synthesis process, thereby further reducing the size of the synthesized MoS2 nanosheets. The statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 3.8nm. The small size of the MoS2 nanosheets gives it abundant edge sulfur vacancies, thus showing high activity and high selectivity.
[0046] Comparative Example 1
[0047] 1235.9 mg of ammonium molybdate tetrahydrate and 2283.6 mg of thiourea were dissolved and dispersed in 35 mL of deionized water to form a uniform solution. The solution was then packaged in a 100 mL reactor and reacted at 400 °C for 4 hours. The product was -1 The product was stirred in a potassium hydroxide solution at 60°C for 3 hours, washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C. It is recorded as MoS2-5.
[0048] According to XRD characterization, MoS2-5 is a typical 2H-MoS2 structure, and the catalyst does not contain a carrier or template. According to TEM characterization, MoS2-5 is flower-shaped as a whole, and its MoS2 nanosheets have large horizontal line dimensions. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is >100nm. The large size of MoS2 nanosheets makes it lack edge sulfur vacancies, thus showing relatively low selectivity for high-carbon alcohols.
[0049] Comparative Example 2
[0050] 900 mg of ammonium molybdate tetrahydrate and 10 mL of carbon disulfide were placed in a 40 mL stainless steel autoclave under argon protection and reacted at 400 °C for 4 hours. -1 The product was stirred in a potassium hydroxide solution at 60°C for 3 hours, washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C. It is recorded as MoS2-6.
[0051] According to XRD characterization, MoS2-6 is a typical 2H-MoS2 structure, and the catalyst does not contain a carrier or a template. Since no carrier and no solvent were introduced, ammonium molybdate could not be effectively dispersed during the high-temperature synthesis process. According to TEM characterization, MoS2-6 is aggregated as a whole, and its MoS2 nanosheets have a large horizontal dimension. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is >30nm. The large size of MoS2 nanosheets makes it lack edge sulfur vacancies, thus showing relatively low selectivity for high-carbon alcohols.
[0052] Comparative Example 3
[0053] 900 mg of ammonium molybdate tetrahydrate was dissolved in 20 mL of deionized water to form a uniform solution. The above solution and 10 mL of carbon disulfide were then packaged in a 40 mL stainless steel autoclave under argon protection and reacted at 400 °C for 4 hours. The product was -1 The product was stirred in a potassium hydroxide solution at 60°C for 3 hours, washed with anhydrous ethanol and deionized water until neutral, and then dried in an oven at 80°C. It is recorded as MoS2-7.
[0054] According to XRD characterization, MoS2-7 is a typical 2H-MoS2 structure, and the catalyst does not contain a carrier or template. According to TEM characterization, MoS2-7 is flower-shaped as a whole, and its MoS2 nanosheets have large horizontal line dimensions. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is >20nm. The large size of MoS2 nanosheets makes it lack edge sulfur vacancies, thus showing relatively low selectivity for high-carbon alcohols.
[0055] Comparative Example 4
[0056] 1600 mg of ammonium molybdate tetrahydrate and 2500 mg of SBA-15 (pore inner diameter of about 6-13 nm) were dispersed in 100 mL of deionized water, then stirred to dry at room temperature and dried in an oven at 80 ° C overnight. The dried sample was packaged in a 100 mL stainless steel autoclave with 40 mL of carbon disulfide under argon protection and reacted at 500 ° C for 12 hours. The product was treated in a hydrofluoric acid solution at room temperature for 8 hours to remove the SBA-15 template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80 ° C. It is recorded as MoS2-8.
[0057] According to XRD characterization, MoS2-8 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed, and the MoS2-8 catalyst does not contain a carrier or a template agent. According to TEM characterization, although MoS2-8 can replicate part of the SBA-15 template, most of the MoS2 nanosheets are still separated from the original SBA-15 structure and appear aggregated, causing the original pores to be blocked. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is about 4nm. Although the size of the nanosheets in MoS2-8 is close to that of MoS2-2, it does not have a complete one-dimensional ordered linear structure, and most of the pores are blocked, resulting in the diffusion of reactants, products and intermediate molecules in the pores being restricted, so the activity and selectivity of high-carbon alcohols are much lower than those of MoS2-2.
[0058] Comparative Example 5
[0059] 1600 mg of ammonium molybdate tetrahydrate was physically mixed with 2500 mg of SBA-15 (pore inner diameter of about 6-13 nm), and the mixed sample was packaged with 40 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon protection and reacted at 500 ° C for 12 hours. The product was treated in a hydrofluoric acid solution at room temperature for 8 hours to remove the SBA-15 template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80 ° C. It is recorded as MoS2-9.
[0060] According to XRD characterization, MoS2-9 is a typical 2H-MoS2 structure, and there is no XRD signal of silicon dioxide, indicating that the template has been completely removed, and the MoS2-9 catalyst does not contain a carrier or a template agent. According to TEM characterization, MoS2-9 hardly replicates the pore structure of the SBA-15 template, and the MoS2 nanosheets are aggregated. The statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 4nm. Although the size of the nanosheets in MoS2-9 is close to that of MoS2-2, because the MoS2 nanosheets are aggregated and do not have a complete one-dimensional ordered linear structure, the diffusion of reactants, products and intermediate molecules is restricted, so the activity and selectivity of high-carbon alcohols are much lower than those of MoS2-2.
[0061] Comparative Example 6
[0062] 1200 mg of ammonium molybdate was physically mixed with 5333 mg of silica sphere dispersion (ethylene glycol dispersion containing 30 wt% silica, silica sphere diameter of about 100-200 nm). The mixed sample was packaged with 20 mL of carbon disulfide in a 100 mL stainless steel autoclave under argon protection and reacted at 450 ° C for 6 hours. The resulting product was treated in a potassium hydroxide solution at 80 ° C for 24 hours to remove the silica template, then washed with anhydrous ethanol and deionized water to neutrality, and then dried in an oven at 80 ° C. It was recorded as MoS2-10.
[0063] According to XRD characterization, MoS2-10 is a typical 2H-MoS2 structure, and there is no XRD signal of silica, indicating that the template has been completely removed, and the MoS2-10 catalyst does not contain a carrier or a template. According to TEM characterization, MoS2-10 hardly replicates the pore structure of the silica template, and the MoS2 nanosheets are aggregated. The statistical results based on TEM characterization show that the average size of the MoS2 nanosheets is about 6.5nm. Although the size of the nanosheets in MoS2-10 is close to that of MoS2-1, the MoS2 nanosheets are aggregated and do not have a complete three-dimensional macroporous structure, which limits the diffusion of reactants, products and intermediate molecules, so the activity and selectivity of high-carbon alcohols are much lower than those of MoS2-1.
[0064] Comparative Example 7
[0065] Commercial molybdenum disulfide (CAS No.: 1317-33-5) was used as a comparative sample and recorded as MoS2-11.
[0066] According to XRD characterization, MoS2-11 is a typical 2H-MoS2 structure with high crystallinity and no carrier or template. According to TEM characterization, MoS2-11 presents a large lamellar structure. The statistical results based on TEM characterization show that the average size of MoS2 nanosheets is >200nm. The large size of MoS2 nanosheets makes it lack edge sulfur vacancies, thus showing relatively low selectivity for high-carbon alcohols.
[0067] Comparison
[0068] The MoS2-based catalyst used in the present invention completely replicates the pores of SBA-15 and SiO2 balls to form a multi-scale pore structure. According to the comparison of MoS2-2 with MoS2-8 and MoS2-9 of the present invention; and the comparison of MoS2-1 with MoS2-10, it can be clearly seen that the multi-scale pore structure formed after the complete replication of the template plays an important role in improving the catalyst activity and the selectivity of high-carbon alcohols. In addition, through the performance comparison of a series of MoS2-based catalysts modified with different alkali metals, the K-modified MoS2-based catalyst prepared with potassium carbonate or potassium hydroxide as an auxiliary agent has better performance, and the performance is better when the molar ratio of K / Mo is 0.2.
[0069] The method of adding alkali metal is:
[0070] The above MoS2-1 to 11 were ultrasonically dispersed in 50 mL of deionized water for 3 hours, and then an appropriate amount of alkali metal salt or hydroxide solution was added, and ultrasonic dispersion was continued for 3 hours. Then, the mixture was stirred to dryness at room temperature and dried at 80°C to obtain alkali metal-modified MoS2 samples, which were respectively recorded as Cat-XYZ, where X corresponds to MoS2-1 to 11, Y is the alkali metal salt or hydroxide used, and Z is the molar content ratio of the alkali metal / Mo used.
[0071] The catalysts in Table 1 all use potassium carbonate as an auxiliary agent, and the K / Mo molar ratio is 0.2, so they are abbreviated as Cat-1 to Cat-11.
[0072] MoS2-2 was ultrasonically dispersed in 50 mL of deionized water for 3 hours, and then an appropriate amount of alkali metal salt or hydroxide solution shown in Table 2 was added and ultrasonic dispersion was continued for 3 hours. The mixture was then stirred to dryness at room temperature and dried at 80°C to obtain an alkali metal-modified MoS2-2 sample.
[0073] MoS2-2 was ultrasonically dispersed in 50 mL of deionized water for 3 hours, and then different amounts of potassium carbonate solution in Table 3 were added and ultrasonically dispersed for another 3 hours. The mixture was then stirred to dryness at room temperature and dried at 80°C to obtain the alkali metal-modified MoS2-2 sample.
[0074] The application of the catalyst takes a fixed bed reactor as an example, and the specific steps are as follows:
[0075] Before filling the catalyst, the catalyst was first molded into particles of 250-600 μm. Then 200 mg of catalyst was loaded into the reaction tube and then 1 bar, 30 mL min -1 H2 was pretreated at 300℃ for 1 hour. When the temperature dropped to the reaction temperature (240℃ for example), the reaction gas was switched to CO / H2 with a ratio of 1 / 2 (containing 4% Ar as an internal standard substance to calculate the CO conversion rate) and pressurized to 50 bar. The reaction gas space velocity was 3000 mL gcat. -1 h -1 For example, the reaction product was analyzed online by gas chromatograph, and TCD and FID detectors were used for qualitative and quantitative analysis respectively. The specific reaction performance is listed in Table 1.
[0076] Table 1 Catalyst performance evaluation results
[0077]
[0078] Table 2 Properties of MoS2-2 samples modified with different alkali metals
[0079]
[0080] Note: The molar ratio of alkali metal to Mo is 0.2
[0081] Table 3 Properties of MoS2-2 samples modified with different potassium carbonate contents
[0082]
Claims
1. A catalyst for preparing higher alcohols from synthesis gas, characterized in that: The catalyst is a small-sized, multi-scale porous molybdenum sulfide material modified by an alkali metal, which has abundant sulfur vacancies at the edge of molybdenum sulfide; the porous channel skeleton of the porous molybdenum sulfide material is formed by molybdenum sulfide itself; the size of the nanosheet of the molybdenum sulfide material is 0.5 to 15 nm; The multi-scale porous structure is composed of micropores of 0.2 to 2 nm between molybdenum sulfide nanosheets and mesopores, macropores or both formed by the support of the molybdenum sulfide nanosheet skeleton, and the inner diameter of the pores is 2 to 1000 nm; the mesopores or macropores are at least one of one-dimensional linear pores, two-dimensional linear cross pores or three-dimensional spherical pores.
2. The catalyst for preparing higher alcohols from synthesis gas according to claim 1, characterized in that: The average pore size of mesopores or macropores is 6 to 400 nm.
3. A method for preparing the catalyst according to claim 1 or 2, characterized in that: By selecting a suitable template A, the molybdenum source B is uniformly dispersed on the template A or the template A* after surface treatment, and then the sulfur source C is introduced, and the molybdenum source B and the sulfur source C are reacted in situ at high temperature to obtain a reaction product D in a one-step method, and then the reaction product D is transferred to a post-treatment liquid E for treatment to wash away the template, and the small-sized, multi-scale porous molybdenum sulfide material F is obtained by suction filtration and washing, and the molybdenum sulfide material F is uniformly mixed with an alkali metal additive G to obtain a synthesis gas to high-carbon alcohol catalyst H; the method for uniformly dispersing the molybdenum source B on the template A or the template A* after surface treatment is at least one of an ultrasonic dispersion method, a mixed grinding method, and a ball milling method; The alkali metal auxiliary agent G is at least one of potassium hydroxide or metal salt compounds.
4. The method for preparing the catalyst according to claim 3, characterized in that The template A is at least one of silica spheres, silica nanowires, SBA-15, KIT-6, alumina nanowires, titanium oxide nanowires, titanium oxide nanospheres, and titanium oxide nanotubes, and the diameters of the above-mentioned oxide spheres, oxide nanowires, and oxide nanotubes are 2 to 400 nm; the molybdenum source B is at least one of ammonium molybdate, sodium molybdate, potassium molybdate, phosphomolybdic acid, sodium phosphomolybdate, potassium phosphomolybdate, molybdenum chloride, and molybdenum acetylacetonate; the sulfur source C is thiourea, sulfur, sodium sulfide, potassium sulfide, hydrogen sulfide, ammonium tetrathiomolybdate, carbon disulfide, dimethyl sulfoxide, thioacetamide, cysteine, At least one of methionine and thiol; the molar ratio of molybdenum atoms to sulfur atoms in the molybdenum source B and the sulfur source C is 1:1 to 1:500; the catalyst synthesis temperature is 180 to 600°C, and the synthesis time is 0.5 to 48 hours; the post-treatment liquid E is at least one of hydrofluoric acid solution, sulfuric acid solution, hydrochloric acid solution, nitric acid solution, sodium hydroxide solution, potassium hydroxide solution, and ammonia solution; the post-treatment time is 0.5 to 48 hours; the alkali metal additive G is potassium carbonate or potassium hydroxide; the molar ratio of the alkali metal additive G to the alkali metal atoms in molybdenum sulfide to the molybdenum atoms is 0.02 to 5.
5. The method for preparing the catalyst according to claim 3, characterized in that The method for obtaining the template A* through surface treatment is at least one of hydroxylation, amination, carboxylation and alkylation.
6. The method for preparing the catalyst according to claim 3, characterized in that The method for uniformly dispersing the molybdenum source B on the template A or the surface-treated template A* is at least one of ultrasonic dispersion, mixed grinding and ball milling. The ultrasonic frequency is 10 to 300 kHz. The specific steps of the ultrasonic dispersion method are: (1) first add the template A or A* into a dispersant, and ultrasonically disperse for 0.5 to 6 hours. The dispersant is water, methanol, ethanol, propanol, acetone, or a mixed solution thereof; the concentration of the template and the dispersant to form a dispersion is 1 g / L to 1000 g / L; (2) add the molybdenum source B into the above dispersion, and ultrasonically disperse for 0.5 to 6 hours. The specific steps of the mixed grinding method are: mixing the template A or A* and the molybdenum source B in a mortar, and mixing and grinding for 0.5 to 6 hours. The specific steps of the ball milling method are: mixing the template A or A* and the molybdenum source B in a ball milling jar, placing the ball milling jar on a ball mill for 2 to 50 hours. The material of the ball milling jar is at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and hard alloy; the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, or hard alloy balls; the ball-to-material ratio is 200:1 to 10:1 (mass ratio); the ball milling speed is 200 to 1500 rpm.
7. The method for preparing the catalyst according to claim 3, characterized in that The molybdenum sulfide material F and the alkali metal additive G are mixed by at least one of a liquid phase dispersion stirring method, a mixed grinding method, and a ball milling method; The specific steps of the liquid phase dispersion and stirring method are: (1) dissolving the alkali metal additive G in a solvent to form a solution, wherein the solvent is at least one of water, methanol, ethanol, acetone, and N,N-dimethylformamide (DMF); (2) adding the molybdenum sulfide material F to the above solution, and ultrasonically dispersing for 0.5 to 6 hours to form a dispersion; (3) placing the above dispersion at 25 to 150° C. and stirring until dry, thereby achieving uniform mixing of the molybdenum sulfide material F and the alkali metal additive G. The ultrasonic frequency is 10 to 300 kHz; The specific steps of the mixed grinding method are: mixing the molybdenum sulfide material F and the alkali metal additive G in a mortar, and mixing and grinding for 0.5 to 6 hours; The specific steps of the ball milling method are: mixing the molybdenum sulfide material F and the alkali metal additive G in a ball milling jar, placing the ball milling jar on a ball mill for 2 to 50 hours. The material of the ball milling jar is at least one of polytetrafluoroethylene, zirconium oxide, stainless steel, agate, and hard alloy; the ball milling balls are at least one of zirconium oxide balls, stainless steel balls, agate balls, or hard alloy balls; the ball-to-material ratio is 200:1 to 10:1 (mass ratio); the ball milling speed is 200 to 1500 rpm.
8. Use of the catalyst according to claim 1 or 2 in the reaction of synthesizing higher alcohols from synthesis gas, characterized in that: The catalyst is used for preparing high-carbon alcohols from synthesis gas and is suitable for one or more of a fixed bed reactor, a fluidized bed reactor, a moving bed reactor, a slurry bed reactor and a kettle reactor.
9. Use of the catalyst according to claim 8 in the reaction of synthesizing higher alcohols from synthesis gas, characterized in that: The catalyst is pretreated at 180-600°C for 0.5-50 hours in an inert atmosphere, a reducing atmosphere or a mixed atmosphere of the two before being used in the synthesis gas to prepare higher carbon alcohol reaction; the inert atmosphere is at least one of nitrogen, argon, helium and neon; the reducing atmosphere is at least one of hydrogen, carbon monoxide and hydrogen sulfide; the synthesis gas atmosphere is at least one of CO / H2 and CO / CO2 / H2; the higher carbon alcohol is at least one of alcohols containing more than 2 carbon atoms.
Citation Information
Patent Citations
Carbon-supported catalysts for production of higher alcohols from syngas
CN103313785A
Deep hydrodesulfurization catalyst for oil product and preparation method of deep hydrodesulfurization catalyst
CN108568309A
Molybdenum disulfide with three-dimensional hierarchical pore structure and preparation method and application thereof
CN111841579A
High-efficiency non-noble metal water electrolysis catalytic material as well as preparation method and application thereof
CN113058619A
Preparation method of hydrodesulfurization catalyst with mesoporous carbon material as carrier
CN113893867A