Novel high-efficiency gas phase fluorination catalyst and preparation method thereof

By roasting aluminum oxide powder, amorphous chromium oxide powder, organic matter, graphite and other materials, the problem of poor activity and stability of the gas-phase fluorination catalyst in high-temperature treatment is solved, the high specific surface area and pore structure are maintained, and the efficiency is improved. Catalyst activity and life.

CN118807793AInactive Publication Date: 2024-10-22SHAANXI NAVIS INNOVATIVE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410707288.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing gas-phase fluorination catalysts have problems such as high exothermic phenomena during the fluorination activation process, resulting in increased catalyst grains, reduced specific surface area, low activity, poor stability, and frequent reactivation.

Method used

The mixing and roasting treatment method of alumina powder, amorphous chromium oxide powder, organic matter, graphite and other materials is used to maintain the high specific surface area and pore structure of the catalyst after high temperature treatment, prevent excessive precipitation of precipitated particles, and create pores through the volatilization of organic matter. , improve the activity and life of the catalyst.

Benefits of technology

It achieves a high specific surface area and rich pore structure of the catalyst, maintains high activity and long life, and avoids the problems of reduced catalyst activity and poor stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807793A_ABST
    Figure CN118807793A_ABST
Patent Text Reader

Abstract

The invention discloses a novel high-efficiency gas-phase fluorination catalyst and a preparation method thereof, and relates to the technical field of fluorination catalysts, the novel high-efficiency gas-phase fluorination catalyst comprises alumina powder, amorphous chromium oxide powder, an organic matter 1, graphite and absolute ethyl alcohol, the materials are mixed and uniformly shaken, and the mixture is roasted and fluorinated after being uniformly shaken to obtain the gas-phase fluorination catalyst. Under the combined action of the aluminum oxide powder, the amorphous chromic oxide powder and the organic matter 1, precipitation particles can be highly dispersed, excessive precipitation of the precipitation particles in the precipitation process is prevented, on the one hand, in the roasting stage, the organic matter 1 is heated and volatilized, the pore forming effect is achieved, and meanwhile the collapse rate of pore channels can be effectively reduced; the synergistic effect of the two is beneficial for the catalyst to still maintain high specific surface area, original pore diameter and morphology after high-temperature treatment, the catalyst can be decomposed and volatilized by heating to play a pore-forming role and a lubricating and bonding role, the activity of the gas-phase fluorination catalyst is improved, the service life of the gas-phase fluorination catalyst is prolonged, and the catalyst has the characteristics of high specific surface area and rich pore structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fluorination catalysts, and in particular to a novel high-efficiency gas-phase fluorination catalyst and a preparation method thereof. Background Art

[0002] Gas-phase fluorination catalysts are the core of the process route for producing fluorocarbons, and gas-phase fluorination catalysts mainly use chromium-based solid catalysts or aluminum-based solid catalysts; a large number of studies have found that the catalytic activity of fluorination catalysts is closely related to the pore volume, pore size and specific surface area of ​​the catalyst. Generally speaking, high specific surface area, high pore volume and appropriate pore size can effectively improve the activity and selectivity of the catalyst. Gas-phase fluorination catalysts only show high catalytic activity and high selectivity in the fluorinated state, but the precursor of the gas-phase fluorination catalyst mainly exists in the form of oxides, not in the fluorinated state. Therefore, the precursor of the gas-phase fluorination catalyst needs to be fluorinated before the reaction. The high exothermic phenomenon during the fluorination activation treatment directly leads to the increase of catalyst grains and a significant reduction in specific surface area, resulting in low activity, poor stability and frequent regeneration and activation of the fluorination catalyst. Therefore, there is an urgent need for a high-temperature resistant, high-specific surface area gas-phase fluorination catalyst, which is of great significance. Summary of the invention

[0003] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0004] A novel high-efficiency gas-phase fluorination catalyst comprises aluminum oxide powder, amorphous chromium oxide powder, organic matter 1, graphite and anhydrous ethanol. The above materials are mixed and shaken evenly, and then calcined and fluorinated to obtain the gas-phase fluorination catalyst.

[0005] A method for preparing a novel high-efficiency gas-phase fluorination catalyst comprises the following steps:

[0006] Step 1: Selection of experimental tools;

[0007] Step 2: Material selection and weighing;

[0008] Step 3: Mix and stir;

[0009] Step 4: Filtration, washing and drying;

[0010] Step 5: Calcination.

[0011] A further improvement of the technical solution of the present invention is that: in the step 1, multiple volumetric flasks, magnetic stirrers, electronic balances, multiple beakers and laboratory ovens need to be prepared in advance, and after the experimental equipment is selected, each experimental equipment needs to be disinfected with alcohol disinfectant to avoid affecting the purity of the subsequent preparation of the gas-phase fluorination catalyst.

[0012] A further improvement of the technical solution of the present invention is that: in the step 2, aluminum oxide powder, amorphous chromium oxide powder, organic matter 1, graphite and anhydrous ethanol need to be selected, and an electronic balance needs to be used to weigh 8 grams of aluminum oxide powder, 12 grams of amorphous chromium oxide powder, 5 grams of organic matter 1 and 3 grams of graphite respectively, and 20 milliliters of anhydrous ethanol is measured with a volumetric flask.

[0013] A further improvement of the technical solution of the present invention is that: in step three, an empty volumetric flask is selected, 8 grams of aluminum oxide powder, 12 grams of amorphous chromium oxide powder, 5 grams of organic matter 1, 3 grams of graphite and 20 milliliters of anhydrous ethanol in step two are poured into the volumetric flask, and finally stirred by using a prepared magnetic stirrer until all the raw materials are fully blended, at which time the stirring is stopped to obtain a gas-phase fluorination catalyst solution.

[0014] A further improvement of the technical solution of the present invention is that: the solution obtained in step three is first filtered through a laboratory filtering device, a few drops of precipitant solution are added to the solution before the filtering process, and then it is washed, and finally it is placed in a prepared laboratory oven, the drying temperature is controlled to 80-100 degrees, and the drying is carried out for 50 minutes, thereby obtaining a solid dry product.

[0015] The further improvement of the technical solution of the present invention is that: the step 5 is to calcine the dried product in step 4, during which nitrogen needs to be continuously added, the calcination temperature is 200-350 degrees, and the calcination time is 2 hours. After the calcination, a gas-phase fluorination catalyst with high purity can be obtained.

[0016] Due to the adoption of the above technical solution, the present invention has the following technical advances compared with the prior art:

[0017] 1. The present invention provides a novel method for preparing a high-efficiency gas-phase fluorination catalyst. Through the joint action of alumina powder, amorphous chromium oxide powder and organic matter 1, the precipitated particles can be highly dispersed to prevent excessive precipitation of the precipitated particles during the precipitation process. On the other hand, in the calcination stage, the organic matter 1 is volatilized by heat to play a pore-forming role, and at the same time, the pore collapse rate can be effectively reduced; the synergistic effect of the two is conducive to the catalyst still maintaining a high specific surface area, original pore size and morphology after high-temperature treatment, and can be thermally decomposed and volatilized to play a pore-forming role and lubrication and bonding role, thereby improving the activity and life of the gas-phase fluorination catalyst. The catalyst has the characteristics of high specific surface area and rich pore structure, so this gas-phase fluorination catalyst has good activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The present invention is a flow chart of a method for preparing a novel high-efficiency gas-phase fluorination catalyst. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with embodiments:

[0020] Example 1

[0021] like Figure 1 As shown, the present invention provides a novel high-efficiency gas-phase fluorination catalyst, including aluminum oxide powder, amorphous chromium oxide powder, organic matter 1, graphite and anhydrous ethanol. The above materials are mixed and shaken evenly, and then calcined and fluorinated to obtain a gas-phase fluorination catalyst.

[0022] Example 2

[0023] like Figure 1 As shown, the present invention provides a method for preparing a novel high-efficiency gas-phase fluorination catalyst, comprising the following steps:

[0024] Step 1: Selection of experimental tools;

[0025] Step 2: Material selection and weighing;

[0026] Step 3: Mix and stir;

[0027] Step 4: Filtration, washing and drying;

[0028] Step 5: Calcination.

[0029] Example 3

[0030] like Figure 1As shown, on the basis of Example 2, the present invention provides a technical solution: preferably, in step one, multiple volumetric flasks, magnetic stirrers, electronic balances, multiple beakers and laboratory ovens need to be prepared in advance, and each experimental instrument needs to be disinfected with an alcohol disinfectant after the experimental instruments are selected to avoid affecting the purity of the subsequent preparation of the gas-phase fluorination catalyst. In step two, aluminum oxide powder, amorphous chromium oxide powder, organic matter 1, graphite and anhydrous ethanol need to be selected. Here, an electronic balance is used to weigh 8 grams of aluminum oxide powder, 12 grams of amorphous chromium oxide powder, 5 grams of organic matter 1 and 3 grams of graphite, and 20 milliliters of anhydrous ethanol is measured with a volumetric flask. In step three, an empty volumetric flask is selected, and 8 grams of aluminum oxide powder, 12 grams of amorphous chromium oxide powder, 5 grams of organic matter 1, 3 grams of graphite and 20 milliliters of anhydrous ethanol are all poured into a volumetric flask, and finally stirred by using a prepared magnetic stirrer until all raw materials are fully fused, and then the stirring stops to obtain a gas phase fluorination catalyst solution, and the solution obtained in step 3 is first filtered through a laboratory filtration device, and a few drops of precipitant solution need to be added to the solution before the filtration process, and then washed, and finally placed in a prepared laboratory oven, the drying temperature is controlled to be 80-100 degrees, and the drying process is 50 minutes, so as to obtain a solid dry product, and step 5 is to roast the dried product in step 4, and nitrogen needs to be continuously added during this process, and the roasting temperature is 200-350 degrees, and the roasting time is 2 hours. After roasting, a gas phase fluorination catalyst with higher purity can be obtained.

[0031] In this embodiment, the precipitated particles can be highly dispersed to prevent excessive precipitation of the precipitated particles during the precipitation process. On the other hand, during the calcination stage, the organic matter 1 is volatilized by heat to play a pore-forming role, and at the same time, the pore collapse rate can be effectively reduced; the synergistic effect of the two is beneficial for the catalyst to maintain a high specific surface area, original pore size and morphology after high-temperature treatment, and can be thermally decomposed and volatilized to play a pore-forming role and lubrication and adhesion role, thereby improving the activity and life of the gas-phase fluorination catalyst. The catalyst has the characteristics of high specific surface area and rich pore structure, so this gas-phase fluorination catalyst has good activity.

[0032] The above generally describes the present invention in detail, but it is obvious to a person skilled in the art that some modifications or improvements can be made to the present invention. Therefore, modifications or improvements that do not depart from the spirit of the present invention are within the scope of protection of the present invention.

Claims

1. A novel high-efficiency gas-phase fluorination catalyst, comprising aluminum oxide powder, amorphous chromium oxide powder, organic matter 1, graphite and anhydrous ethanol, characterized in that: The above materials are mixed and shaken evenly, and then calcined and fluorinated to obtain a gas phase fluorination catalyst.

2. The method for preparing a novel high-efficiency gas-phase fluorination catalyst according to claim 1, characterized in that: The following steps are involved: Step 1: Selection of experimental tools; Step 2: Material selection and weighing; Step 3: Mix and stir; Step 4: Filtration, washing and drying; Step 5: Calcination.

3. The method for preparing a novel high-efficiency gas-phase fluorination catalyst according to claim 2, characterized in that: In the step 1, multiple volumetric flasks, magnetic stirrers, electronic balances, multiple beakers and laboratory ovens need to be prepared in advance. After the experimental equipment is selected, each experimental equipment needs to be disinfected with alcohol disinfectant to avoid affecting the purity of the subsequent preparation of the gas-phase fluorination catalyst.

4. The method for preparing a novel high-efficiency gas-phase fluorination catalyst according to claim 2, characterized in that: In the step 2, aluminum oxide powder, amorphous chromium oxide powder, organic matter 1, graphite and anhydrous ethanol need to be selected. Here, an electronic balance needs to be used to weigh 8 grams of aluminum oxide powder, 12 grams of amorphous chromium oxide powder, 5 grams of organic matter 1 and 3 grams of graphite respectively, and 20 milliliters of anhydrous ethanol is measured with a volumetric flask.

5. The method for preparing a novel high-efficiency gas-phase fluorination catalyst according to claim 2, characterized in that: The step three is to select an empty volumetric flask, pour 8 grams of aluminum oxide powder, 12 grams of amorphous chromium oxide powder, 5 grams of organic matter 1, 3 grams of graphite and 20 milliliters of anhydrous ethanol in the step two into the volumetric flask, and finally stir it by using the prepared magnetic stirrer until all the raw materials are fully blended, at which time the stirring is stopped to obtain a gas-phase fluorination catalyst solution.

6. The method for preparing a novel high-efficiency gas-phase fluorination catalyst according to claim 2, characterized in that: The solution obtained in step three is first filtered through a laboratory filtering device. Before the filtering process, a few drops of precipitant solution are added to the solution, and then it is washed. Finally, it is placed in a prepared laboratory oven, the drying temperature is controlled to be 80-100 degrees, and the drying is carried out for 50 minutes to obtain a solid dry product.

7. The method for preparing a novel high-efficiency gas-phase fluorination catalyst according to claim 2, characterized in that: The step five is to calcine the dried product in step four, during which nitrogen needs to be continuously added, the calcination temperature is 200-350 degrees, and the calcination time is 2 hours. After calcination, a gas-phase fluorination catalyst with high purity can be obtained.