Preparation method and application of N-Zn0. 5Cd0. 5S photocatalytic material for degrading imidacloprid pesticide

By preparing N-Zn0.5Cd0.5S composite photocatalyst, nitrogen doping technology is used to solve the problem of low imidacloprid degradation efficiency in the existing technology, and achieve efficient and environmentally friendly pesticide residue degradation effect, which is suitable for large-scale industrial applications.

CN118807804APending Publication Date: 2024-10-22INNER MONGOLIA UNIVERSITY

Patent Information

Application Number
CN202410724920.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing technologies have problems with highly toxic materials and corrosiveness when degrading imidacloprid residues, and the wide bandgap of ZnS limits its photocatalytic performance, making it difficult to effectively decompose pesticide residues.

Method used

The N-Zn0.5Cd0.5S composite photocatalyst is prepared through hydrothermal method and nitrogen doping technology to adjust the band gap width and increase the active sites on the catalyst surface to improve the photocatalytic performance.

Benefits of technology

The degradation efficiency of imidacloprid is significantly improved under sunlight conditions. The degradation rate of 92.6% exceeds the 16.5% of undoped materials. It is simple to operate, low in cost, and has potential for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention designs a preparation method of a nitrogen-doped modified Zn0. 5Cd0. 5S photocatalyst capable of degrading imidacloprid pesticides. According to the preparation method, environment-friendly ammonium citrate is used as a nitrogen source, nitrogen is introduced into Zn0. 5Cd0. 5S crystal lattices by adopting a hydrothermal method, the nitrogen doping amount is controlled by adjusting the dosage of the ammonium citrate, then the defect energy level and the electron distribution state are adjusted, and the nitrogen-doped modified Zn0. 5Cd0. 5S photocatalyst is obtained. The separation of photo-induced electrons and holes is promoted, and the absorption spectrum moves towards the direction of visible light, so that the utilization efficiency of solar energy is improved. The prepared N-Zn0. 5Cd0. 5S material can degrade 92.6% of 10 mg / L imidacloprid under the irradiation of visible light for 180 min, and the activity is superior to that of other similar products. The preparation method is simple, the nitrogen doping amount is easy to control, and the prepared N-Zn0. 5Cd0. 5S semiconductor photocatalytic material is high in catalytic efficiency, capable of degrading imidacloprid in the natural environment, easy to operate, free of secondary pollution, high in cost performance and wide in application prospect in the field of pesticide residue treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of pesticide residue management and environmental safety, and specifically relates to a preparation method and application of a semiconductor photocatalytic material for degrading residual pesticides. Background Art

[0002] Imidacloprid (IMC) is the most widely used pesticide among neonicotinoid insecticides. It is often used to protect economic crops such as vegetables, tea trees and fruit trees. Compared with other insecticides, imidacloprid has high toxicity to target pests and low toxicity to mammals, which has increased people's use of imidacloprid. However, residual pesticides may form harmful intermediates under environmental influences, posing a threat to humans and the environment.

[0003] Photocatalytic degradation has always been an effective method to reduce imidacloprid residues in food and the environment, and has become an efficient, eco-friendly and low-cost technology. CdS has been widely studied in the field of photocatalysis due to its suitable band gap and appropriate visible light response, but its application is limited by unfavorable factors such as its high toxicity and susceptibility to photocorrosion. In addition, ZnS can quickly generate electron-hole pairs and has excellent catalytic activity under ultraviolet light. However, its wide band gap of 3.6-3.8 eV is the main factor hindering its photocatalytic performance. Recently, ZnS, which is obtained by replacing part of Cd with Zn, has been studied. x Cd 1-x The solid solution of S has attracted the attention of researchers because compared with single metal sulfide, Zn x Cd 1-x The nanocrystalline structure of the S solid solution has the advantages of narrow band gap and high oxidation potential. By further doping with non-metallic N elements, the band gap width is adjusted and defect energy levels are generated, the active sites and active mechanisms on the catalyst surface are increased, and the photogenerated electrons and holes are efficiently separated in space, thereby increasing the catalytic performance.

[0004] The present invention prepares N-Zn 0.5 Cd 0.5 S composite photocatalyst and applied to decompose the pesticide imidacloprid under sunlight conditions. Summary of the invention

[0005] The present invention aims to provide an N-doped ZnO2-doped nanostructured carbon nanotube for visible light catalytic degradation of imidacloprid under economic and environmentally friendly conditions. 0.5 Cd 0.5 The preparation method of S semiconductor photocatalytic material specifically comprises the following steps: Step 1: Zn 0.5 Cd 0.5 Preparation of S (abbreviated as ZCS): Zinc acetate, cadmium acetate and thioacetamide were mixed in a certain proportion and dispersed in deionized water to obtain dispersion A. Then 4 mol·L -1 Alkali solution B is added dropwise into dispersion A, and after sufficient dispersion and mixing, a reaction solution C is obtained. The reaction solution C is charged into a high-pressure reactor for a constant-temperature hydrothermal reaction. After the reaction is completed, it is naturally cooled to room temperature, and a yellow product is collected by centrifugation. The product is washed alternately with deionized water and ethanol, and dried to obtain ZCS. Step 2: N-doped Zn 0.5 Cd 0.5 Preparation of S (abbreviated as NZCS): Ammonium citrate was added to the dispersion A in the above step 1 until it was fully dissolved, and then a certain concentration of alkali solution B was prepared, and the alkali solution B was added dropwise to the dispersion A containing ammonium citrate to obtain a reaction solution D. The reaction solution D was charged into a high-pressure reactor to perform a constant temperature hydrothermal reaction. After the reaction was completed, it was naturally cooled to room temperature, and a yellow product was collected by centrifugation. It was washed alternately with deionized water and ethanol, and dried to obtain N-Zn 0.5 Cd 0.5 S catalyst, the samples were marked as NZCS-n according to the amount of ammonium citrate added (when the amount of ammonium citrate added was 0.1, 0.5, 1.0, 2.0, 3.0 g, they were named NZCS-1, NZCS-2, NZCS-3, NZCS-4, NZCS-5, respectively); Step 3: Evaluate the degradation activity of imidacloprid Add 20 mg NZCS-n catalyst and 40 mL 10 mg·L -1 The imidacloprid solution was photocatalytically degraded using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 minutes. Samples were taken every 60 minutes and centrifuged to obtain the supernatant. The concentration change was measured using a UV-visible spectrophotometer to evaluate the decomposition activity of imidacloprid.

[0006] In step 1, the molar ratio of zinc acetate, cadmium acetate and thioacetamide is 1:1:2, and the amount of deionized water is 30-50 mL.

[0007] In steps 1 and 2, the temperature of the isothermal hydrothermal reaction is 170-190 °C, and the isothermal time is 20-25 h.

[0008] In steps 1 and 2, the drying temperature is 50-60°C and the drying time is 5-10 h.

[0009] In step 2, the amount of ammonium citrate added is 0.1~3 g.

[0010] The beneficial effects of the present invention are: (1) The present invention uses environmentally friendly and mild ammonium citrate as a nitrogen source and prepares N-Zn by a simple hydrothermal method. 0.5 Cd 0.5 The S-3 composite catalyst can degrade 10 mg / L imidacloprid by 92.6% under visible light irradiation for 180 min, which is 16.5% higher than the degradation efficiency of undoped single-phase ZCS, making the degradation more complete and thorough.

[0011] (2) The catalyst of the present invention is simply doped with nitrogen and is combined with Zn 0.5 Cd 0.5 The S solid solutions act synergistically to increase the active sites on the catalyst surface, effectively realizing the separation of photogenerated carriers. The doped structure effectively reduces its band gap width and improves the utilization rate of visible light, thereby increasing the catalytic activity of the nanocomposite material.

[0012] (3) The catalyst preparation process of the present invention is simple to operate, has high catalytic activity, does not require complex equipment, and uses low-cost raw materials. The imidacloprid degradation reaction can occur under sunlight. It is simple to operate, has high activity, and has no secondary pollution. It has the potential for large-scale industrial preparation and industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 (a) is the X-ray powder diffraction spectrum of CdS, ZCS and ZnS, where the main diffraction peaks of CdS are located at 26.56°, 43.87° and 52.0°, respectively, corresponding to the CdS cubic phase with JCPDS card number 89-0440; the main diffraction peaks of ZnS are located at 28.55°, 47.48° and 56.35°, corresponding to the sphalerite phase of ZnS with JCPDS card number 65-1961; the main diffraction peaks of CdS and ZnS can be observed in the XRD spectrum of the ZCS sample, indicating the successful preparation of the solid solution; Figure 1 (b) is the X-ray powder diffraction spectrum of ZCS with different nitrogen doping levels. With the increase of N doping amount, the characteristic diffraction peak shifts significantly and finally exists as three main diffraction peaks. This is mainly due to the lattice expansion phenomenon after N doping.

[0014] Figure 2 (a) and (b) are scanning electron microscope images of ZCS and NZCS-3, respectively, and (c) is a transmission electron microscope image of NZCS-3. The test results show that both ZCS and NZCS-3 present relatively uniform spherical nanoparticles, so the doping of N does not change the characteristic morphology and microstructure of ZCS.

[0015] Figure 3X-ray photoelectron spectra of ZCS and NZCS-3 samples, (a) 2p orbital of Zn, (b) 3d orbital of Cd, (c) 2p orbital of S, and (d) 1s orbital of N.

[0016] Figure 4 (a) A series of N-doped ZCS catalysts with different ratios degraded 10 mg·L -1 The catalytic activity of imidacloprid was shown in Figure 4 (b). NZCS-3 was able to degrade 92.6% of imidacloprid under visible light irradiation in 180 min, and the undoped pure phase ZCS degraded 76.1% of imidacloprid in 180 min. -1 Changes in the absorbance of imidacloprid under the action of NZCS-3 catalyst: As the illumination time increases, the characteristic absorption peak of imidacloprid gradually weakens.

[0017] Figure 5 UV-visible diffuse reflectance spectra of ZCS and NZCS-3 samples. The results show that the absorption edge of N-doped ZCS red-shifts from 520 nm to 530 nm compared with pure ZCS, and the band gap of NZCS-3 is reduced from 2.39 eV of ZCS to 2.35 eV, indicating that the absorption range of light is expanded after doping, and more visible light can be used for catalytic reactions.

[0018] Figure 6 (a) Photocurrent response and (b) electrochemical impedance of ZCS and NZCS-3. The test results show that NZCS-3 has stronger light response characteristics and smaller charge transfer resistance than ZCS, indicating that the probability of photogenerated carrier recombination in the nitrogen-doped material is low and the charge separation efficiency is enhanced, making the NZCS-3 material show higher photocatalytic degradation activity of imidacloprid under visible light than pure ZCS catalyst. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with specific embodiments. Example 1

[0020] Preparation of ZCS: Weigh 1.10 g zinc acetate (Zn(Ac) 2 ·2H 2 O), 1.33 g cadmium acetate (Cd(Ac) 2 ·2H 2 O) and 0.93 g thioacetamide were dispersed in 40 mL deionized water and stirred until dissolved to obtain dispersion A. Subsequently, 10 mL 4 mol·L -1The NaOH aqueous solution is recorded as alkali solution B. Alkali solution B is added dropwise into dispersion A, and after stirring and dispersing evenly, dispersion C is obtained. Dispersion C is placed in a high-pressure reactor and maintained at 180 °C for 24 h. After the reaction is completed, it is naturally cooled to room temperature, and a yellow product is obtained by centrifugation. It is washed alternately with deionized water and ethanol, and dried at 60 °C.

[0021] ZCS photocatalytic degradation performance test of imidacloprid: In a 50 mL quartz tube, add 20 mg ZCS catalyst and 40 mL 10 mg·L -1 The imidacloprid solution was photocatalytically degraded using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 minutes. Samples were taken every 60 minutes and centrifuged to obtain the supernatant, and its concentration change was measured using a UV-visible spectrophotometer. The degradation rate of imidacloprid was 76.1% within 180 minutes. Example 2

[0022] Preparation of NZCS-1: Weigh 1.10 g zinc acetate (Zn(Ac) 2 ·2H 2 O), 1.33 g cadmium acetate (Cd(Ac) 2 ·2H 2 O) and 0.93 g thioacetamide were dispersed in 40 mL deionized water and stirred until dissolved to obtain dispersion A. 0.1 g ammonium citrate was added to dispersion A and stirred thoroughly to dissolve. Then 10 mL 4 mol·L -1 The NaOH aqueous solution is denoted as alkali solution B. Alkali solution B is added dropwise into dispersion A, and after stirring and dispersing evenly, dispersion D is obtained. Dispersion D is placed in a high-pressure reactor and maintained at 180 °C for 24 h. After the reaction is completed, it is naturally cooled to room temperature, and a yellow product is collected by centrifugation. It is washed alternately with deionized water and ethanol, and dried at 60 °C to obtain NZCS-1.

[0023] NZCS-1 photocatalytic degradation performance test of imidacloprid: In a 50 mL quartz tube, add 20 mg ZCS catalyst and 40 mL 10 mg·L -1 The imidacloprid solution was photocatalytically degraded using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 minutes. Samples were taken every 60 minutes and centrifuged to obtain the supernatant, and its concentration change was measured using a UV-visible spectrophotometer. The degradation rate of imidacloprid was 83.3% within 180 minutes. Example 3

[0024] Preparation of NZCS-2: Weigh 1.10 g zinc acetate (Zn(Ac) 2 ·2H2 O), 1.33 g cadmium acetate (Cd(Ac) 2 ·2H 2 O) and 0.93 g thioacetamide were dispersed in 40 mL deionized water and stirred until dissolved to obtain dispersion A. 0.5 g ammonium citrate was added to dispersion A and stirred thoroughly to dissolve. Then 10 mL 4 mol·L -1 The NaOH aqueous solution is denoted as alkali solution B. Alkali solution B is added dropwise into dispersion A, and after stirring and dispersing evenly, dispersion D is obtained. Dispersion D is charged into a high-pressure reactor and maintained at 180 °C for 24 h. After the reaction is completed, it is naturally cooled to room temperature, and a yellow product is collected by centrifugation. It is washed alternately with deionized water and ethanol, and dried at 60 °C to obtain NZCS-2.

[0025] NZCS-2 photocatalytic degradation performance test of imidacloprid: In a 50 mL quartz tube, add 20 mg ZCS catalyst and 40 mL 10 mg·L -1 The imidacloprid solution was photocatalytically degraded using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 minutes. Samples were taken every 60 minutes and centrifuged to obtain the supernatant, and its concentration change was measured using a UV-visible spectrophotometer. The degradation rate of imidacloprid was 90.1% within 180 minutes. Example 4

[0026] Preparation of NZCS-3: Weigh 1.10 g zinc acetate (Zn(Ac) 2 ·2H 2 O), 1.33 g cadmium acetate (Cd(Ac) 2 ·2H 2 O) and 0.93 g of thioacetamide were dispersed in 40 mL of deionized water and stirred until dissolved to obtain dispersion A. 1.0 g of ammonium citrate was added to dispersion A and stirred thoroughly to dissolve. Then 10 mL of 4 mol·L -1 The NaOH aqueous solution is denoted as alkali solution B. Alkali solution B is added dropwise into dispersion A, and after stirring and dispersing evenly, dispersion D is obtained. Dispersion D is charged into a high-pressure reactor and maintained at 180 °C for 24 h. After the reaction is completed, it is naturally cooled to room temperature, and a yellow product is collected by centrifugation. It is washed alternately with deionized water and ethanol, and dried at 60 °C to obtain NZCS-3.

[0027] NZCS-3 photocatalytic degradation performance test of imidacloprid: Add 20 mg of NZCS-3 catalyst and 40 mL of 10 mg·L -1The imidacloprid solution was photocatalytically degraded using visible light as the light source. The dark reaction lasted for 60 minutes and then the light was turned on after reaching the adsorption-desorption equilibrium. Samples were taken every 60 minutes and centrifuged to obtain the supernatant, and its concentration change was measured using a UV-visible spectrophotometer. The degradation rate of imidacloprid was 92.6% within 180 minutes. Example 5

[0028] Preparation of NZCS-4: Weigh 1.10 g zinc acetate (Zn(Ac) 2 ·2H 2 O), 1.33 g cadmium acetate (Cd(Ac) 2 ·2H 2 O) and 0.93 g of thioacetamide were dispersed in 40 mL of deionized water and stirred until dissolved to obtain dispersion A. 2.0 g of ammonium citrate was added to dispersion A and stirred thoroughly to dissolve. Then 10 mL of 4 mol·L -1 NaOH aqueous solution was added to obtain dispersion B, which was loaded into a high-pressure reactor and maintained at 180 °C for 24 h. After the reaction was completed, it was naturally cooled to room temperature and collected by centrifugation to obtain a yellow product, which was washed alternately with deionized water and ethanol and dried at 60 °C to obtain NZCS-4.

[0029] NZCS-4 photocatalytic degradation performance test of imidacloprid: 20 mg NZCS-4 catalyst and 40 mL 10 mg / L imidacloprid solution were added to a 50 mL quartz tube, and photocatalytic degradation was carried out using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 min. Samples were taken every 60 min and centrifuged to obtain the supernatant, and its concentration change was measured using a UV-visible spectrophotometer. The degradation rate of imidacloprid was 73.8% within 180 min. Example 6

[0030] Preparation of NZCS-5: Weigh 1.10 g zinc acetate (Zn(Ac) 2 ·2H 2 O), 1.33 g cadmium acetate (Cd(Ac) 2 ·2H 2 O) and 0.93 g of thioacetamide were dispersed in 40 mL of deionized water and stirred until dissolved to obtain dispersion A. 3 g of ammonium citrate was added to dispersion A and stirred thoroughly to dissolve. Then 10 mL of 4 mol·L -1The NaOH aqueous solution is denoted as alkali solution B. Alkali solution B is added dropwise into dispersion A, and after stirring and dispersing evenly, dispersion D is obtained. Dispersion D is placed in a high-pressure reactor and maintained at 180 °C for 24 h. After the reaction is completed, it is naturally cooled to room temperature, and a yellow product is collected by centrifugation. It is washed alternately with deionized water and ethanol, and dried at 60 °C to obtain NZCS-5.

[0031] NZCS-5 photocatalytic degradation performance test of imidacloprid: Add 20 mg of NZCS-5 catalyst and 40 mL of 10 mg·L -1 The imidacloprid solution was photocatalytically degraded using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 minutes. Samples were taken every 60 minutes and centrifuged to obtain the supernatant, and its concentration change was measured using a UV-visible spectrophotometer. The degradation rate of imidacloprid was 61.0% within 180 minutes.

Claims

1. A N-Zn for pesticide degradation 0.5 Cd 0.5 The preparation method and application of S photocatalytic material are characterized in that , follow the steps below: Step 1: Zn 0.5 Cd 0.5 Preparation of S, referred to as ZCS, Zinc acetate, cadmium acetate and thioacetamide were mixed in a molar ratio of 1:1:2 and dispersed in deionized water to obtain dispersion A. Then 10 mL of 4 mol·L -1 Alkali solution B of NaOH was added dropwise to dispersion solution A, and after sufficient dispersion and mixing, a reaction solution C was obtained. The reaction solution C was charged into a high-pressure reactor for a constant temperature hydrothermal reaction at 180 ° C for 24 h. After the reaction was completed, it was naturally cooled to room temperature, and a yellow product was collected by centrifugation, which was washed alternately with deionized water and ethanol, and dried to obtain ZCS; Step 2: N-doped Zn 0.5 Cd 0.5 Preparation of S, referred to as NZCS-n, Different amounts of ammonium citrate were added to the dispersion A in step 1 until it was fully dissolved, and then 10 mL of 4 mol·L -1 The alkali solution B containing NaOH was added dropwise to the dispersion A containing ammonium citrate to obtain a reaction solution D, which was charged into a high-pressure reactor and subjected to a constant temperature solvent thermal reaction at 180 °C for 24 h. After the reaction was completed, it was naturally cooled to room temperature, and a yellow product was collected by centrifugation. The product was washed alternately with deionized water and ethanol, and dried to obtain N-Zn 0.5 Cd 0.5 S catalyst, according to the amount of ammonium citrate added, the samples were marked as NZCS-n, and when the amount of ammonium citrate added was 0.1, 0.5, 1.0, 2.0, and 3.0 g, they were marked as NZCS-1, NZCS-2, NZCS-3, NZCS-4, and NZCS-5, respectively.

2. The nitrogen-doped Zn according to claim 1 0.5 Cd 0.5 The application of NZCS-n material prepared by the preparation method of S solid solution in photocatalytic degradation of imidacloprid is characterized in that: In a 50 mL quartz tube, add 20 mg NZCS-n catalyst and 40 mL 10 mg·L -1 The imidacloprid solution was photocatalytically degraded using visible light as the light source. The light was turned on after the dark reaction reached the adsorption-desorption equilibrium after 60 minutes. Samples were taken every 60 minutes and centrifuged to obtain the supernatant. The concentration change was measured using a UV-visible spectrophotometer to evaluate the decomposition activity of imidacloprid.

3. The method for preparing the catalyst according to claim 1, characterized in that: In step 2, ammonium citrate is used as a nitrogen source to adjust the nitrogen doping amount to prepare a nitrogen-doped NZCS-n catalyst.

4. The use of the catalyst according to claim 2, characterized in that: The prepared NZCS-n materials were used to photocatalytically degrade imidacloprid. NZCS-3 photocatalyzed the degradation of 10 mg·L -1 The degradation rate of imidacloprid was 92.6%.

5. The NZCS-n nanocomposite material obtained by the preparation method according to any one of claims 1 to 4 is used for the purification of neonicotinoid pesticide residues.

Citation Information

Patent Citations

  • Preparation method of nitrogen-doped modified zinc oxide visible-light photocatalyst

    CN111001429A

  • Preparation method of carbon-doped modified zinc oxide visible-light-induced photocatalyst

    CN111036190A

  • Preparation method for CD 0.5zn 0.5s and experimental method for nitrogen fixation under photocatalysis thereof

    WO2023246306A1

Cited By

  • CdZnS-based composite material as well as preparation method and application thereof

    CN120205211A