Preparation method and application of catalyst for preparing gamma-valerolactone through furfural conversion
By simplifying the catalyst preparation process and combining hafnium tetrachloride and heteropoly acid with a silica-based carrier, the problems of low catalyst activity and high cost in the existing technology have been solved, and efficient γ-valerolactone preparation has been achieved. The reaction time is shortened and the selectivity is improved.
Patent Information
- Application Number
- CN202410791918.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the catalyst preparation for preparing γ-valerolactone by converting furfural is complicated, the catalyst activity and selectivity are low, the reaction time is long, and the cost of the precious metal catalyst is high.
Hafnium tetrachloride and heteropoly acid are combined with a silica-based carrier to prepare a bifunctional solid acid catalyst through impregnation, stirring and roasting. The ratio of Lewis acid to acid is adjusted to simplify the catalyst preparation process and be used under appropriate conditions. Furfural conversion reaction.
The high activity and selectivity of the catalyst are achieved, the reaction time is shortened, the cost is reduced, and the yield and selectivity of γ-valerolactone are improved.
Smart Images

Figure CN118807818A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical catalytic materials, and particularly relates to a catalyst for preparing gamma-valerolactone by converting furfural and a preparation method thereof. Background Art
[0002] Due to the depletion of fossil fuels and environmental degradation, research on the catalytic conversion of biomass platform compounds into value-added products has expanded rapidly. Furfural is an abundant, low-cost biomass platform molecule that can be easily produced by dehydration of corn cobs or other lignocellulosic biomass. Furfural can be converted into a variety of value-added compounds through reactions such as hydrogenation, oxidative condensation, oxidative esterification, and ring opening. Among the many products, γ-valerolactone, as a high-value-added chemical, has attracted widespread attention due to its excellent physical and chemical properties. For example, in the food industry, it is often used as a flavor and food additive; in the petrochemical industry, it can be used as a fuel additive and diesel oxygenator; and as a green solvent, it is widely used in a variety of chemical reactions. At present, the production of furfural from corn cobs has been industrialized, so the preparation of γ-valerolactone by furfural conversion is a green and promising process production route.
[0003] At present, a variety of precious metal and zirconium-based catalysts are widely used in the reaction of furfural conversion to prepare γ-valerolactone. For example, in the literature Applied Catalysis B: Environmental 241 (2019) 588-597, HPA / Zr-Beta catalyst was synthesized. After reacting at 160°C for 24 hours, the highest yield of γ-valerolactone obtained under the optimal conditions was only 68%, less than 70%, and the amount of catalyst used was large. The catalyst preparation process was very cumbersome: H-Al-Beta was converted to Si-Beta through dealumination, washing, drying, and calcination; then, Si-Beta was mixed with a zirconium precursor and calcined to form Zr-Beta; finally, heteropolyacid and Zr-Beta were impregnated and calcined to convert into HPA / Zr-Beta catalyst. Although a variety of catalysts have been synthesized for the reaction of furfural conversion to prepare γ-valerolactone, there are still disadvantages such as complex catalyst preparation, high reaction temperature, long reaction time, and low catalyst stability.
[0004] The conversion of furfural to γ-valerolactone involves multiple steps, including carbonyl reduction, ring opening / rearrangement, and lactonization. The carbonyl reduction step can be achieved via the Meerwein-Ponndorf-Verley (MPV) reaction. Using alcohol as the hydrogen donor, the process from furfural to γ-valerolactone can be summarized as follows: under the catalysis of Lewis acid, through catalytic transfer hydrogenation, furfural is first reduced to furfuryl alcohol, and then etherified to furfuryl ether. Then Under acid catalysis, furfuryl ether is converted into alkyl levulinate through a ring-opening reaction, and then the alkyl levulinate is converted into 4-carboxyvalerate through an MPV reaction, and finally 4-carboxyvalerate is converted into γ-valerolactone through lactonization. Based on this, a novel alkyl levulinate with Lewis acid and Acid and Lewis acid and Catalysts with adjustable acid ratios are of great significance for the efficient catalytic conversion of furfural to produce γ-valerolactone. Summary of the invention
[0005] The present invention aims to solve the problems of complicated catalyst preparation, low catalyst activity and selectivity, long reaction time and high price in the current reaction of furfural conversion to prepare γ-valerolactone, and provides a catalyst for furfural conversion to prepare γ-valerolactone and a preparation method thereof. The catalyst designed by the present invention is simple to prepare, and the required bifunctional solid acid catalyst can be obtained by impregnation, stirring and calcination. By adjusting the ratio of heteropoly acid and hafnium chloride, the Lewis acid and The catalyst preparation process of the present invention is simple and can be easily mass-produced.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A preparation method of a catalyst for preparing γ-valerolactone by one-pot conversion of furfural, the method is carried out according to the following steps: weighing a certain mass of hafnium tetrachloride (HfCl4), heteropoly acid (HPA) and silicon oxide-based carrier (SiO2) and adding them into deionized water, stirring at room temperature to obtain a white mixed solution, placing the white mixed solution in an oil bath pot under the condition of 80-120°C and drying to obtain a white solid. Finally, placing it in a muffle furnace, roasting it in an air atmosphere for 4 hours, the roasting temperature is above 400°C, and the catalyst is obtained, which is recorded as HPA / Hf-silicon oxide-based carrier catalyst.
[0008] As a limitation of the present invention, the heteropoly acid selected in the catalyst synthesized by the present invention includes one or more of phosphotungstic acid, phosphomolybdic acid, silicotungstic acid and silicomolybdic acid, preferably phosphotungstic acid (HPW).
[0009] As a limitation of the present invention, the silicon oxide-based carrier selected in the catalyst synthesized in the present invention is a mesoporous all-silicon molecular sieve or an amorphous high specific surface area SiO2; the all-silicon molecular sieve is specifically SBA-15, MCM-41 or FDU-12. SBA-15 is further preferred.
[0010] As a limitation of the present invention, the mass ratio of HPA / HfO2 in the catalyst synthesized by the present invention is 0.1 to 1.3.
[0011] As a limitation of the present invention, HfO2: carrier = 2.5 to 15 wt%.
[0012] As a limitation of the present invention, the calcination temperature needs to be controlled above 400°C, preferably 400°C, at which temperature the performance is higher. If the temperature is lower than 400°C, hafnium tetrachloride cannot be calcined into HfO2, and the effect will be reduced.
[0013] The HPA / Hf-SiO catalyst prepared above is applied in the reaction of furfural conversion to prepare γ-valerolactone according to the following method:
[0014] (1) adding a certain amount of alcohol solvent, HPA / Hf-silica-based carrier catalyst and furfural into a high-pressure reactor;
[0015] (2) After replacing the air with nitrogen three times, fill with nitrogen with an initial pressure of 0.8 MPa, set a certain stirring speed, set the reaction temperature to 150°C to 190°C, and the reaction time to 1 to 15 hours. After the reaction is completed, the reactor is quickly cooled to room temperature, the reaction liquid is filtered, and the product is analyzed by gas chromatography.
[0016] As a limitation of the present invention, the mass ratio of the catalyst to furfural is 0.01 to 0.5.
[0017] As a limitation of the present invention, the selected alcohol solvent is one of ethanol, n-propanol, isopropanol and 2-butanol. The preferred alcohol solvent is isopropanol.
[0018] As a limitation of the present invention, the preferred reaction temperature is 170° C. to 190° C. and the reaction time is 5 to 12 hours.
[0019] After adopting the above technical solution, the present invention achieves the following beneficial effects:
[0020] The invention uses hafnium tetrachloride and heteropoly acid as precursors and silicon oxide-based materials as carriers to prepare a catalyst with precisely adjustable catalytic active sites, high specific surface area and Lewis acid and The acid ratio is adjustable. The main reason for the high catalytic activity of the catalyst of the present invention is that: in the above reaction, the metal Hf acts as a Lewis acid center to catalyze the transfer hydrogenation reaction, which can effectively inhibit other by-products generated by excessive hydrogenation, such as furfural hydrogenation to generate 2-methylfuran and tetrahydrofurfuryl alcohol; HPW is The acid center catalyzes the etherification and ring-opening / rearrangement processes, and the synergistic catalytic effect of the two acids plays a key role in the formation of γ-valerolactone. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The pyridine infrared images of the catalysts of Examples 1-4 show that each catalyst contains Lewis and Acid center.
[0022] Figure 2 It is the SEM and TEM images of the HPW / Hf-SBA-15_0.4 catalyst obtained in Example 2; it can be seen from the figure that after HfO2 and HPW are loaded on SBA-15, the skeleton structure of SBA-15 is not destroyed. In addition, it can be seen that HfO2 and HPW are uniformly dispersed on the surface of SBA-15. DETAILED DESCRIPTION
[0023] The present invention will be further described with respect to the following examples, but it should be understood that these examples are only for illustration purposes and should not be construed as limitations on the implementation of the present invention. The substances used in the following examples are all conventional commercially available products. Amorphous high specific surface area SiO2 was purchased from Aladdin, SBA-15 and MCM-41 were purchased from Tianjin Nanhua Catalyst Co., Ltd., and FDU-12 was purchased from Taizhou Juna New Energy Co., Ltd.
[0024] The present invention adopts conventional impregnation and high temperature calcination method to synthesize HPA / Hf-silicon oxide based carrier catalyst. Different catalysts can be obtained by adjusting the types of silicon oxide based carrier and heteropoly acid, and the mass ratio of heteropoly acid to hafnium chloride during the synthesis process.
[0025] Examples 1-5
[0026] Effects of different silica-based carrier types on the conversion of furfural to γ-valerolactone. The heteropolyacid is phosphotungstic acid (HPW), the mass ratio of HPW / HfO2 is 0.4 (measured by ICP), and the specific steps are as follows:
[0027] Preparation scheme of HPW / Hf-silica carrier_0.4 catalyst: Weigh 1g silica-based carrier, 0.18g hafnium chloride, and 0.059g phosphotungstic acid (HPW) and add them to 30mL deionized water and stir for 30min. After stopping stirring, the solution is placed in an oil bath and dried at 80℃ until solid. Finally, the solid powder is placed in a muffle furnace and calcined at 400℃ for 4h at a heating rate of 10℃ / min in an air atmosphere to obtain a HPW / Hf-silica carrier_0.4 catalyst with a W / Hf mass ratio of 0.4 (measured by ICP).
[0028] Catalyst performance evaluation plan: Weigh 2mmol furfural, 100mg catalyst and 10mL isopropanol and add them to a 50mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8MPa. Set the reaction temperature to 160℃ and stir the reaction for 5h. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0029] Table 1 Effect of silica-based carrier type on the reaction of furfural conversion to γ-valerolactone
[0030] Example Silica-based carrier Furfural conversion rate (%) γ-Valerolactone selectivity (%) 1 <![CDATA[SiO2]]> 98.2 54.3 2 SBA-15 99.7 62.2 3 MCM-41 99.2 59.7 4 FDU-12 99.8 60.5
[0031] It can be seen from Table 1 that the catalysts synthesized with different silica carriers have good catalytic effects on the conversion of furfural to prepare γ-valerolactone. When SBA-15 is selected as the carrier, the conversion rate of furfural and the selectivity of γ-valerolactone are the highest.
[0032] Embodiment 6-8
[0033] Effects of different heteropolyacids on the conversion of furfural to γ-valerolactone. The silica carrier is SBA-15, the mass ratio of HPA / Hf is 0.4 (measured by ICP), and the specific steps are as follows:
[0034] Preparation scheme of HPA / Hf-SBA-15_0.4 catalyst: Weigh 1g SBA-15, 0.18g hafnium chloride, and 0.059g heteropoly acid and add them to 30mL deionized water and stir for 30min. After stopping stirring, the solution is placed in an oil bath and dried at 80°C until solid. Finally, the solid powder is placed in a muffle furnace and calcined at 400°C for 4h at a heating rate of 10°C / min in an air atmosphere to obtain a HPA / Hf-SBA-15_0.4 catalyst with a W(Mo) / Hf mass ratio of 0.4 (measured by ICP).
[0035] Catalyst performance evaluation plan: Weigh 2mmol furfural, 100mg catalyst and 10mL isopropanol and add them to a 50mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8MPa. Set the reaction temperature to 160℃ and stir the reaction for 5h. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0036] Table 2 Effect of heteropolyacid types on the conversion of furfural to γ-valerolactone
[0037] Example Heteropoly Acid (HPA) Furfural conversion rate (%) γ-Valerolactone selectivity (%) 2 Phosphotungstic acid(HPW) 99.7 62.2 5 Phosphomolybdic acid(HPMo) 100 53.3 6 Silicate Tungstic Acid(HSiW) 99.8 55.6 7 Silicomolybdic acid (HSiMo) 100 53.1
[0038] It can be seen from Table 2 that the catalysts synthesized with different heteropoly acids have good catalytic effects on the conversion of furfural to prepare γ-valerolactone. When phosphotungstic acid is used, the conversion rate of furfural and the selectivity of γ-valerolactone are the highest.
[0039] Examples 9-11
[0040] The effect of W / Hf mass ratio on the conversion of furfural to prepare γ-valerolactone. The silica carrier is SBA-15, the heteropoly acid is HPW, and the specific steps are as follows:
[0041] Preparation scheme of HPW / Hf-SBA-15_x catalyst: Weigh 1g SBA-15, a certain mass of hafnium chloride, and a certain mass of heteropoly acid, add them to 30mL of deionized water and stir for 30min. After stopping stirring, the solution is placed in an oil bath and dried at 80℃ until solid. Finally, the solid powder is placed in a muffle furnace and calcined at 400℃ for 4h at a heating rate of 10℃ / min in an air atmosphere to obtain a HPW / Hf-SBA-15_x catalyst with a W / Hf mass ratio of x (measured by ICP).
[0042] Catalyst performance evaluation plan: Weigh 2mmol furfural, 100mg catalyst and 10mL isopropanol and add them to a 50mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8MPa. Set the reaction temperature to 160℃ and stir the reaction for 5h. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0043] Table 3 Effect of W / Hf mass ratio on the conversion of furfural to γ-valerolactone
[0044]
[0045] It can be seen from Table 3 that different W / Hf mass ratios have good catalytic effects on the conversion of furfural to prepare γ-valerolactone. When the W / Hf mass ratio is 0.4, the conversion rate of furfural and the selectivity of γ-valerolactone are the highest.
[0046] The catalysts used in the following examples (12-26) are all HPW / Hf-SBA-15_0.4, and the specific preparation process of the catalyst is the same as that of Example 2.
[0047] Examples 12-14
[0048] The effect of different reaction temperatures on the conversion of furfural to prepare γ-valerolactone is as follows:
[0049] Weigh 2 mmol furfural, 100 mg HPW / Hf-SBA-15_0.4 and 10 mL isopropanol and add them into a 50 mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8 MPa. Set the reaction temperature to 150-190°C and stir the reaction for 5 hours. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0050] Table 4 Effect of reaction temperature on the conversion of furfural to produce γ-valerolactone
[0051] Example Reaction temperature (℃) Furfural conversion rate (%) γ-Valerolactone selectivity (%) 11 150 98.9 44.2 2 160 99.7 62.2 12 170 99.7 70.9 13 190 99.9 77.4
[0052] Examples 15-18
[0053] The effect of different reaction times on the conversion of furfural to prepare γ-valerolactone is as follows:
[0054] Weigh 2 mmol furfural, 100 mg HPW / Hf-SBA-15_0.4 and 10 mL isopropanol and add them into a 50 mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8 MPa. Set the reaction temperature to 170°C and stir the reaction for 1 to 12 hours. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0055] Table 5 Effect of reaction time on the conversion of furfural to prepare γ-valerolactone
[0056] Example Reaction time (h) Furfural conversion rate (%) γ-Valerolactone selectivity (%) 14 1 99.1 22.2 15 3 99.5 63.9 12 5 99.7 70.9 16 8 99.9 82.5 17 12 100 90.1 18 15 100 91.5
[0057] Examples 20-22
[0058] The effect of different catalyst qualities on the reaction of furfural conversion to prepare γ-valerolactone is as follows:
[0059] Weigh 2 mmol furfural, 10-100 mg HPW / Hf-SBA-15_0.4 and 10 mL isopropanol and add them into a 50 mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8 MPa. Set the reaction temperature to 170°C and stir the reaction for 12 hours. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0060] Table 6 Effect of catalyst quality on the conversion of furfural to γ-valerolactone
[0061] Example Catalyst mass (mg) Furfural conversion rate (%) γ-Valerolactone selectivity (%) 19 10 99.2 29.5 20 50 99.5 60.4 21 70 99.7 79.7 17 100 100 90.1
[0062] Embodiment 23-25
[0063] The effects of different solvents (hydrogen donors) on the reaction of furfural conversion to prepare γ-valerolactone are as follows:
[0064] Weigh 2 mmol furfural, 100 mg HPW / Hf-SBA-15_0.4 and 10 mL solvent and add them into a 50 mL intermittent high-pressure reactor. Replace the gas with nitrogen three times and then fill it with nitrogen with an initial pressure of 0.8 MPa. Set the reaction temperature to 170°C and stir the reaction for 12 hours. After the reaction, the product analysis is carried out quantitatively by gas chromatography.
[0065] Table 7 Effect of solvent (hydrogen donor) on the reaction of furfural conversion to γ-valerolactone
[0066] Example Solvents Furfural conversion rate (%) γ-Valerolactone selectivity (%) 22 Ethanol 98.2 68.2 23 n-Propanol 99.2 75.4 17 Isopropyl alcohol 100 90.1 24 2-Butanol 99.8 88.7
[0067] It can be seen from Tables 4-7 that reaction conditions such as reaction temperature, time, catalyst quality, and solvent have a great influence on the reaction, but the conversion rate of furfural can reach more than 95%. Under appropriate reaction conditions (170°C, 12h, 100mg catalyst, isopropanol as solvent), the selectivity of γ-valerolactone reaches more than 90%.
[0068] Embodiment 26
[0069] The same conditions as those in Applied Catalysis B:Environmental 241(2019)588-597
[0070] Catalyst performance evaluation scheme: 1.1mmol furfural, 1.056mg HPW / Hf-SBA-15_0.4 catalyst (prepared by the same method as in Example 2) and 20mL isopropanol were weighed and added to a 50mL intermittent autoclave, the gas was replaced with nitrogen three times and then filled with nitrogen with an initial pressure of 1.0MPa, the reaction temperature was set to 160°C, the reaction was stirred for 24h, and the product analysis after the reaction was completed was quantitatively analyzed by gas chromatography. The conversion rate of furfural was 100%, and the selectivity of GVL was 92.8%.
[0071] By comparing with the comparative literature (Applied Catalysis B: Environmental 241 (2019) 588-597), it is found that under the same reaction conditions (amount of raw materials, amount of catalyst, temperature, time), the HPW / Hf-SBA-15_0.4 catalyst exhibits better catalytic performance. The present invention significantly improves the yield of γ-valerolactone; when the conversion rate of furfural and the selectivity of γ-valerolactone are comparable to those of the prior art, the reaction temperature of the present invention is lower and the reaction time is shorter. The catalyst of the present invention exhibits excellent catalytic performance for the reaction of furfural conversion to prepare γ-valerolactone.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a catalyst for converting furfural into γ-valerolactone, characterized in that: Weigh hafnium tetrachloride, heteropoly acid and silica-based carrier, add into deionized water, stir at room temperature to obtain a white mixed solution, place the white mixed solution in an oil bath, dry under heating conditions to obtain a white solid, place the white solid in a muffle furnace, and calcine at above 400° C. in an air atmosphere to obtain a catalyst, recorded as HPA / Hf-silica-based carrier; the mass ratio of HPA and HfO2 in the catalyst is 0.1-1.3; the silica-based carrier is a mesoporous all-silica molecular sieve or amorphous SiO2.
2. The method for preparing a catalyst for furfural conversion to gamma-valerolactone according to claim 1, characterized in that: The selected heteropolyacid includes one or more of phosphotungstic acid, phosphomolybdic acid, silicotungstic acid and silicomolybdic acid.
3. The method for preparing a catalyst for furfural conversion to gamma-valerolactone according to claim 1, characterized in that: The mesoporous all-silica molecular sieve is one of SBA-15, MCM-41 or FDU-12.
4. The method for preparing a catalyst for converting furfural into γ-valerolactone according to claim 1, characterized in that: The content of HfO2 in the catalyst is 2-10wt%.
5. The method for preparing a catalyst for converting furfural into γ-valerolactone according to claim 1, characterized in that: The heteropoly acid is phosphotungstic acid; the silica-based carrier is SBA-15; and the mass ratio of HPA / HfO2 is 0.
4.
6. Use of the catalyst prepared according to the method according to any one of claims 1 to 5 in the preparation of γ-valerolactone by conversion of furfural, characterized in that: (1) adding furfural, HPA / Hf-silica-based carrier catalyst and alcohol solvent into a high-pressure reactor; (2) After replacing the air with nitrogen, fill in nitrogen with an initial pressure of 0.8 MPa. Under stirring, set the reaction temperature to 150°C to 190°C and the reaction time to 1 to 15 hours. After the reaction is completed, quickly cool the reactor to room temperature and filter to obtain the reaction liquid.
7. The use according to claim 6, characterized in that: The mass ratio of HPA / Hf-silicon oxide based carrier catalyst to furfural is 0.01 to 0.
5.
8. The use according to claim 6, characterized in that: The alcohol solvent is one of ethanol, n-propanol, isopropanol and 2-butanol.
9. The use according to claim 6, characterized in that: The reaction temperature is 170°C to 190°C, and the reaction time is 5 to 12 hours.
10. The use according to claim 6, characterized in that: The alcohol solvent is isopropyl alcohol.
Citation Information
Cited By
Method for preparing gamma-valerolactone through one-pot two-step catalysis of xylose
CN119775231A
Preparation method and application of double-site catalyst
CN120790230A