Preparation method of MOFs catalyst for ethylene oligomerization reaction

By modifying MOFs with sulfonic acid to construct a bifunctional catalyst, the problem of insufficient catalytic activity and selectivity for ethylene oligomerization in the existing technology is solved, and high activity and selectivity are achieved under unsupported catalyst conditions at room temperature. Reduced operating costs and environmental pressure.

CN118807845APending Publication Date: 2024-10-22CHINA UNIV OF PETROLEUM (BEIJING)

Patent Information

Application Number
CN202410826437.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing ethylene oligomerization catalysts have deficiencies in catalytic activity and product selectivity, and the use of cocatalysts will increase operating costs, safety risks, and environmental pressure.

Method used

By modifying metal organic framework materials (MOFs) with sulfonic acid and introducing sulfamic acid or 1,3-propanethiol as a modifying reagent, a bifunctional catalyst for ethylene oligomerization can be constructed to reduce or eliminate the need for cocatalysts. rely.

Benefits of technology

The ethylene oligomerization catalytic activity and product selectivity are significantly improved. The catalyst can exhibit high activity and excellent selectivity at room temperature without the need for a cocatalyst. The catalytic activity is increased nearly ten times, and the C8 selectivity reaches more than 70.32%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910632000000051
    Figure BDA0004910632000000051
  • Figure BDA0004910632000000052
    Figure BDA0004910632000000052
  • Figure BDA0004910632000000053
    Figure BDA0004910632000000053
Patent Text Reader

Abstract

The invention discloses a preparation method of an ethylene oligomerization MOFs catalyst. The method comprises the following step: performing sulfonic acid modification on the metal organic framework material to obtain the metal organic framework material. In order to improve ethylene oligomerization activity and product selectivity at low temperature under the condition of not using a cocatalyst, a sulfonic acid group is introduced into MOFs with unsaturated metal L acid site as B acid, and the MOFs bifunctional catalyst for ethylene oligomerization is constructed. The ethylene oligomerization activity of the bifunctional catalysts at low temperature without a cocatalyst is obviously higher than that of intrinsic MOFs; especially for 10SA / MMIL-101 (Cr), the activity of the catalyst can reach 21953 g / (mol (Cr). H), and the C8 selectivity of the catalyst can reach 70.32%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a method for preparing an ethylene oligomerization reaction MOFs catalyst. Background Art

[0002] Polymerization of light olefins into higher quality large carbon olefins is an important method for producing high-value gasoline, diesel, synthetic lubricants, surfactants, polyolefins and other important industrial products. Among them, ethylene polymerization has been commercialized for decades. Due to its advantages of simple process, high product quality and low pollution, its proportion in the olefin industry has been expanding year by year. The reported ethylene polymerization catalysts mainly include zeolites, non-metallocene catalysts and MOFs.

[0003] In recent years, bifunctional catalysts formed by loading metal ions into zeolites have achieved the polymerization of ethylene without the action of co-catalysts. The polymerization activity of ethylene can reach 63.2g / (g(cat.)·h). These reactions are generally carried out at a high temperature of about 200°C. After the reaction, these catalysts can be easily separated and recovered, but the selectivity of the polymers is poor, which hinders the application of such catalysts in industry. Non-metallocene catalysts can effectively catalyze the polymerization of ethylene in the presence of co-catalysts such as methylamine and alkylaluminum. These catalysts show high catalytic activity and product selectivity. For example, the ethylene oligomerization activity of nickel-based non-metallocene catalysts exceeds 10 7 g / (mol(Ni)·h), the dimerization selectivity reaches more than 85%. For chromium-based non-metallocene catalysts, the ethylene oligomerization activity exceeds 10 6 g / (mol(Ni)·h), the selectivity of trimerization or tetramerization reaches more than 60%. However, the separation and recovery of such catalysts are challenging. In addition, a large amount of MAO, alkyl aluminum or other co-catalysts are required to obtain high catalytic activity, with the Al / metal molar ratio in the range of 300-2000. The widespread use of these co-catalysts will lead to increased operating costs, safety risks and environmental pressures.

[0004] As a class of porous materials, MOFs are also widely used in ethylene oligomerization because of their advantages of multiple modification methods and precise control of catalytic active sites. When catalyzing the reaction, they can be easily separated from the product and reused. However, the use of MAO or alkyl aluminum or other co-catalysts in this system is also inevitable, and its activity is 1-2 orders of magnitude lower than that of non-metallocene catalyst systems. In order to reduce the use of co-catalysts, some researchers have conducted some pioneering studies. For example, Stennett et al. reported a new chromium (III) species containing a weakly coordinating anion [Al(OC4F9)4] for selective ethylene oligomerization. -. In combination with N,N-bis(diarylphosphino)amine "PNP" ligands and a small amount of alkylaluminum AlMe3, the required activation dose of alkylaluminum can be reduced by 30 times. Yeh et al. dripped a Ni aqueous solution with a volume equivalent to the pore volume of UiO-66 into a suspension containing UiO-64 hexane, reduced the nitrate at a temperature of 523K, and obtained a unique catalyst system containing Ni active sites. When the catalyst was activated in helium at 573K for 4h, it could catalyze ethylene dimerization without the use of a co-catalyst, and the catalytic activity reached 200g / (mol(Ni)h) at 1MPa. Despite the above-mentioned partial improvements, the catalytic activity or product selectivity still needs to be further improved when using MOFs as catalysts for ethylene polymerization. Summary of the invention

[0005] In view of the defects in the prior art, the present invention provides a method for preparing an ethylene oligomerization reaction MOFs catalyst.

[0006] The preparation method of the MOFs catalyst for ethylene oligomerization provided by the present invention comprises the following steps: modifying a metal organic framework material (MOFs) with sulfonic acid to obtain the MOFs catalyst.

[0007] Preferably, the metal organic framework material is a MOFs having unsaturated metal Lewis acid sites, and specifically can be selected from at least one of the following: MIL-101(Cr), UiO-66-NH2, MIL-101(Cr)-NH2.

[0008] The above metal organic framework material can be prepared by the method disclosed in the prior art, or obtained through commercial channels.

[0009] Preferably, the modification agent used in the sulfonic acid modification is aminosulfonic acid (SA) or 1,3-propanethiol.

[0010] According to one embodiment of the present invention, MIL-101(Cr) is subjected to sulfonic acid modification, and the modified agent used is aminosulfonic acid (SA).

[0011] The specific modification method is as follows: dissolving aminosulfonic acid in deionized water, and then adding MIL-101(Cr) thereto; vigorously stirring the obtained suspension for 2-6 hours, and immersing for 8-16 hours to obtain SA / MIL-101(Cr).

[0012] Preferably, the method further comprises the following steps: washing the obtained SA / MIL-101(Cr) with deionized water and drying.

[0013] In the above method, the mass percentage of aminosulfonic acid to MIL-101(Cr) is x%, and the value range of x% is 0-90%, preferably -10%-30%.

[0014] In the above method, the drying condition is drying at 100° C. for 12 hours.

[0015] In the above method, the MIL-101(Cr) needs to be degassed before use, and the degassing conditions are: vacuum degassing at 150° C. for 12 hours.

[0016] According to one embodiment of the present invention, UiO-66-NH2 is subjected to sulfonic acid modification, and the modification reagent used is 1,3-propanethiol.

[0017] The specific modification method is as follows: UiO-66-NH2 is dispersed in dichloromethane, and a certain mole of 1,3-propanethiol is added; then the mixture is slowly stirred at 0-40°C for 8-16 hours to obtain UiO-66-NS.

[0018] Preferably, the method further comprises the steps of washing the UiO-66-NS with DMF and dichloromethane and drying.

[0019] In the above method, the feed molar ratio of 1,3-propanethiol to UiO-66-NH2 is x, and the value range of x is 0-8, preferably 4-8.

[0020] In the above method, the drying condition is drying at 60° C. for 12 hours.

[0021] In the above method, the UiO-66-NH2 needs to be degassed before use, and the degassing conditions are: degassing in a vacuum at 80° C. for 3 hours.

[0022] According to one embodiment of the present invention, MIL-101(Cr)-NH2 is subjected to sulfonic acid modification, and the modified agent used is 1,3-propanethiol.

[0023] The specific modification method is as follows: MIL-101(Cr)-NH2 is dispersed in dichloromethane, and a certain mole of 1,3-propanethiol is added; then the mixture is slowly stirred at 0-40°C for 8-16 hours to obtain MIL-101(Cr)-NS.

[0024] Preferably, the method further comprises the following steps: washing the MIL-101(Cr)-NS with DMF and dichloromethane and drying.

[0025] In the above method, the feed molar ratio of 1,3-propanethiol to MIL-101(Cr)-NH2 is x, and the value range of x is 0-8, preferably 4-8.

[0026] In the above method, the drying condition is drying at 60° C. for 12 hours.

[0027] In the above method, the MIL-101(Cr)-NH2 needs to be degassed before use, and the degassing conditions are: degassing in a vacuum at 80° C. for 3 hours.

[0028] The ethylene oligomerization reaction MOFs catalyst prepared by the above method also belongs to the protection scope of the present invention.

[0029] The invention also provides application of the catalyst.

[0030] The application of the catalyst provided by the present invention is the application of the catalyst in catalyzing ethylene oligomerization reaction.

[0031] Preferably, the ethylene oligomerization reaction is carried out at room temperature.

[0032] Preferably, the ethylene oligomerization reaction does not require the addition of any co-catalyst.

[0033] The present invention also provides a method for ethylene oligomerization.

[0034] The method for ethylene oligomerization provided by the present invention comprises the following steps: utilizing the ethylene oligomerization reaction MOFs catalyst provided by the present invention to catalyze ethylene oligomerization reaction.

[0035] Preferably, the temperature of the oligomerization reaction is 15-30° C., the ethylene pressure is 0.5-1.5 MPa; the amount of the catalyst is 10 umoL; and the reaction is carried out in toluene under stirring.

[0036] The present invention prepares three sulfonic acid modified MOFs (SA / MIL-101(Cr), UiO-66-NS and MIL-101(Cr)-NS) in detail and uses them as catalysts for ethylene polymerization at room temperature. They all show excellent catalytic performance without any co-catalyst (e.g., 10SA / MMIL-101(Cr), 21953 g / (mol(Cr)·h), C8 selectivity greater than 70.32%), and their polymerization activity increases nearly tenfold compared with unmodified MOFs. Lewis acid (L acid) and The presence of acid (Br) sites is key to improving performance. In particular, the presence of Br weakens the effects of metal clusters and ligands in MOFs, making it easier for metal centers to combine with ethylene molecules for further oligomerization.

[0037] In order to improve the ethylene polymerization activity and product selectivity at low temperature without using a promoter, the present invention introduces sulfonic acid groups as B acid in MOFs with unsaturated metal L acid sites (i.e., by grafting 1,3-propanethiol on UiO-66-NH2 and MIL-101(Cr)-NH2, respectively, UiO-66-NS and MIL-101(Cr)-NS are obtained), and MOFs bifunctional catalysts for ethylene polymerization are constructed. The ethylene polymerization activity of these bifunctional catalysts at low temperature without a promoter is significantly higher than that of intrinsic MOFs; in particular, for 10SA / MMIL-101(Cr), its activity can reach 21953g / (mol(Cr)·h), and the C8 selectivity can reach 70.32%. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Schematic diagram of ethylene polymerization reaction.

[0039] Figure 2 The catalytic performance of (a) xSA / MMIL-101(Cr) and (b) UiO-66-NSx under the reaction conditions of 25°C, 1 MPa, and 1 h. DETAILED DESCRIPTION

[0040] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.

[0041] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.

[0042] Example 1. Preparation of SA / MIL-101(Cr)

[0043] 6 g of Cr(NO3)3·9H2O and 2.49 g of terephthalic acid were dispersed in 60 mL of deionized water and then ultrasonically dispersed for 20 minutes. The mixture was transferred to a polytetrafluoroethylene-lined autoclave and heated to 218°C for 8 hours. After cooling, the filtered solid was washed once with deionized water, three times with DMF, twice with ethanol, and dried overnight at 100°C. The obtained MIL-101(Cr) was vacuum degassed at 150°C for 12 hours. A certain mass of aminosulfonic acid (m(SA) / m(MIL-101(Cr))=x%, x is 0, 10, 30, 50, 70, 90) was dissolved in 20 mL of deionized water, and then 1 g of degassed MIL-101(Cr) was added. The suspension was vigorously stirred for 4 hours and soaked for 1 day. The filtered solid was washed once with deionized water and dried overnight at 100°C. The obtained green solid was designated as xSA / MIL-101(Cr).

[0044] Example 2. Preparation of UiO-66-NS

[0045] 1.6 g ZrCl4 was added to 150 mL DMF, and 11.4 mL acetic acid was added, and then ultrasonically dispersed until the solid was completely dissolved. 1.2 g 2-aminoterephthalic acid was dissolved in 50 mL DMF. The two solutions were mixed, and 0.5 mL deionized water was added to the mixture. The mixture was transferred to a polytetrafluoroethylene-lined autoclave and heated to 120 ° C for 24 hours. After cooling, the filtered solid was washed three times with DMF, washed twice with ethanol, and dried at 100 ° C overnight. The obtained UiO-66-NH2 was degassed in a vacuum at 80 ° C for 3 hours. 1.5 g of degassed UiO-66-NH2 was dispersed in 20 mL dichloromethane, and a certain mole of 1,3-propanethiol was added, and then the mixture was slowly stirred at 25 ° C for 12 hours. The filtered solid was washed twice with DMF and dichloromethane and dried at 60 ° C overnight. The obtained yellow solid is represented as UiO-66-NSx, wherein x represents the feed molar ratio of 1,3-propanethiol and UiO-66-NH2, and x is 0-8, specifically 0, 1, 2, 4, and 8.

[0046] Example 3. Preparation of MIL-101(Cr)-NS

[0047] 3.2 g Cr(NO3)3·9H2O, 1.44 g 2-aminoterephthalic acid and 0.8 g NaOH were added to 60 mL deionized water and then ultrasonically dispersed for 30 min. The mixture was transferred to a polytetrafluoroethylene-lined autoclave and heated at 150°C for 12 h. After cooling, the filtered solid was washed once with deionized water, three times with DMF, twice with ethanol, and dried at 100°C overnight. The obtained MIL-101(Cr)-NH2 was degassed in a vacuum at 80°C for 3 h. 1 g of degassed MIL-101(Cr)-NH2 was dispersed in 20 mL of dichloromethane, and a certain mole of 1,3-propanethiol was added. The mixture was then slowly stirred at 25°C for 12 h. The filtered solid was washed twice with DMF and dichloromethane and dried at 60°C overnight. The obtained light green solid is represented as MIL-101(Cr)-NSx, wherein x represents the feed molar ratio of 1,3-propanethiol and MIL-101(Cr)-NH2, and x is 0-8, specifically 0, 1, 2, 4, and 8.

[0048] Example 4: Ethylene oligomerization reaction and product characterization

[0049] Ethylene polymerization was carried out using a 250 mL stainless steel autoclave with a mechanical stirrer. The reaction temperature was controlled by a water bath ( Figure 1 ). A certain mass of the catalyst prepared in Example 1-3 and 50 mL of toluene were added to the autoclave, and then the ethylene pressure and temperature were adjusted. After the temperature reached the specified temperature, stirring was started (stirring speed was 100 r / min). After a period of time, stirring was stopped and the reactor was cooled to -15°C. Subsequently, the gas was vented and a small amount of solution was taken for GC analysis. The yield, activity and selectivity of the product were calculated by the following formula.

[0050]

[0051]

[0052]

[0053] Where A0 is the activity of the catalyst for ethylene polymerization, S i Product C i selectivity.

[0054] Catalyst performance characterization:

[0055] 1. With the introduction of sulfonic acid groups, the ethylene catalytic activity of MOFs catalysts is significantly improved.

[0056] In the absence of a promoter, the catalytic activity of MIL-101(Cr) was weak, only 2205 g / (mol(cat.)·h), and the selectivity of C8 was only 48.59%. The catalytic activity of 10SA / MMIL-101(Cr) was as high as 11489 g / (mol(cat.)·h), and the selectivity of C8 was as high as 67.70% (Table 1). After anion exchange in aminosulfonic acid solution, the catalytic activity of 10SA / MMIL-101(Cr) was increased by 5.2 times compared with MIL-101(Cr).

[0057] UiO-66 and UiO-66-NH2 showed low catalytic activity in ethylene polymerization, with catalytic activities of only 940 and 943 g / (mol(cat.)·h), respectively, and C8 selectivity of only 28.99% and 36.78%, respectively. The catalytic activity of UiO-66-NS4 was as high as 13478 g / (mol(cat.)·h), and the C8 selectivity was as high as 68.01%. The catalytic activity of UiO-66-NS4 increased by 14.3 times after modification.

[0058] Table 1 Comparison of ethylene oligomerization activity before and after catalyst modification

[0059]

[0060] Reaction conditions: catalyst 10 μmol (based on MOFs), 25° C., 1 MPa (ethylene), 1 hour, toluene as solvent, GC measurement.

[0061] 2. As the degree of sulfonation of MOFs increases, the selectivity of high-carbon olefin products increases.

[0062] As the degree of sulfonation increases, the catalytic activity of SA / MIL-101(Cr) decreases and the selectivity for C8 increases ( Figure 2 a, Table 2). When sulfonic acid is linked to the backbone of MIL-101(Cr), its terminal -NH3 + The unstable B acid center is formed, which promotes the ethylene polymerization reaction on the Cr center. When the sulfonation of UiO-66-NS reaches saturation, its catalytic activity reaches the maximum value ( Figure 2b, Table 3). The catalytic activity of UiO-66-NS4 is as high as 13472 g / (mol(cat.)·h), and the selectivity of C8 is as high as 68.01%. When the degree of sulfonation continues to increase, the excessive grafted groups occupy the pores, hindering the contact between ethylene and the metal center, and the catalytic activity decreases. However, with the increase of B acid sites, the acid catalytic effect is enhanced, and the selectivity of high carbon olefins above C10 is further improved. When MIL-101(Cr)-NS increases with the increase of B acid sites, the acid catalytic effect is enhanced, and the selectivity of high carbon olefins above C10 is further improved. When the degree of sulfonation reaches saturation, the catalytic activity of MIL-101(Cr)-NS8 is as high as 9010 g / (mol(cat.)·h), which is 3.6 times that of MIL-101(Cr), and the selectivity of C8 is as high as 43.43%( Figure 2 c, Table 4).

[0063] Table 2 Effect of sulfonic acid concentration on the performance of SA / MMIL-101(Cr) catalyst

[0064]

[0065] Reaction conditions: catalyst 10 μmol (based on MOFs), 25 °C, 1 MPa (ethylene), 1 h, toluene as solvent, GC determination. b SA aqueous solution concentration, m(SA) / m(MIL-101(Cr)).

[0066] Table 3 Effect of 1,3-propanethiol equivalent on the catalytic performance of UiO-66-NS

[0067]

[0068]

[0069] a Reaction conditions: catalyst 10 μmol (based on MOFs), 25 °C, 1 MPa (ethylene), 1 h, toluene as solvent, GC determination. b Concentration of 1,3-propanethiol aqueous solution, n(1,3-propanethiol) / n(UiO-66-NH2)

[0070] Table 4 Effect of 1,3-propanethiol equivalent on the catalytic performance of MIL-101(Cr)-NS.

[0071]

[0072] Reaction conditions: catalyst 10 μmol (based on MOFs), 25 °C, 1 MPa (ethylene), 1 h, toluene as solvent, GC determination. b Concentration of 1,3-propanethiol aqueous solution, n(1,3-propanethiol) / n(MIL-101(Cr)-NH2)

[0073] 3. The sulfonic acid modified catalyst SA / MMIL-101(Cr) can obtain higher ethylene polymerization catalytic activity at low temperature and low pressure.

[0074] The catalytic activity of SA / MMIL-101(Cr) increases with the appropriate decrease of ethylene pressure and reaction temperature (Table 5). At 15°C and 1MPa, the catalytic activity of 10SA / MMIL-101(Cr) is as high as 21953g / (mol(cat.)·h), and the selectivity of C8 is as high as 70.32%. The B acid sites introduced by aminosulfonic acid are unstable and can exert better catalytic performance at lower reaction temperatures. With the increase of ethylene pressure and reaction temperature, the reaction rate increases, and the B acid sites are easily separated into solvents, which lose the promoting effect on coordination catalysis. With the increase of reaction temperature and reaction time, the selectivity of higher carbon olefins above C10 is significantly improved. This is because part of the aminosulfonic acid leaves the carrier and enters the solution during the reaction. This part of the aminosulfonic acid acts as an acid catalyst to promote the further conversion of primary oligomerization products into higher carbon olefins.

[0075] Table 5 Effect of reaction temperature and ethylene pressure on the performance of SA / MMIL-101(Cr) catalyst

[0076]

[0077] Reaction conditions: catalyst: 10SA / MMIL-101(Cr), 10 μmol (based on MOFs), 1 hour, toluene as solvent, GC determination.

[0078] 4. As the reaction temperature and pressure increase, the selectivity of high-carbon olefin products of the sulfonic acid-modified catalyst UiO-66-NS increases.

[0079] For the UiO-66-NS catalyst, as the ethylene pressure increases, the concentration of ethylene in the solution increases, resulting in an accelerated reaction rate and an increase in high-carbon olefin products. When the reaction temperature initially increases, the catalytic activity of UiO-66-NS increases, and the high-carbon olefin products increase. However, the solubility of ethylene in the solution decreases with increasing reaction temperature. When the reaction temperature is too high, the solubility of ethylene in the solution is too low, which significantly reduces the reaction rate. On the other hand, the selectivity of high-carbon olefins above C10 increases with increasing reaction temperature. It can be seen that temperature has a great influence on the acid catalytic effect. As the temperature increases, the acid catalytic effect is significantly enhanced, and the carbon number of the product increases. The increase in ethylene pressure leads to an increase in reaction rate and heat release, which also enhances the acid catalytic effect.

[0080] Table 6 Effect of reaction temperature and ethylene pressure on the catalytic performance of UiO-66-NS

[0081]

[0082] Reaction conditions: catalyst: UiO-66-NS4, 10 μmol (based on MOFs), 1 hour, toluene as solvent, GC determination.

[0083] 5. The selectivity of high-carbon olefin products of the sulfonic acid-modified catalyst MIL-101(Cr)-NS increases with the increase of reaction temperature and pressure.

[0084] The catalytic activity of MIL-101(Cr)-NS changes with temperature and pressure similarly to that of UiO-66-NS. However, due to the difference in structure, they show different catalytic performance and stability. The ligands in UiO-66 connect the Zr6O6 clusters into a very stable face-centered cubic structure, and the functional groups on the ligands do not affect the crystallization. In MIL-101-(Cr), the ligands connect the Cr trimers into two groups of cage structures, and the functional groups on the ligands have a great influence on their crystallinity, which greatly affects the catalytic performance of the modified catalyst. As the reaction temperature increases, the catalytic activity of MIL-101(Cr)-NS8 also increases. With the increase of ethylene pressure, the reaction rate and the selectivity of high-carbon olefin products increase. In particular, when MIL-101(Cr)-NS8 was catalyzed at 25°C and 1.5MPa for 1h, the reaction solution became very viscous, and a white to slightly yellow solid precipitated during cooling, which melted into a viscous liquid at room temperature, indicating that a large amount of C14-C18 olefins and aromatic products were produced. MIL-101(Cr)-NS8 was difficult to crystallize, resulting in a large number of sulfonic acid groups exposed to the outside, which greatly improved the acid catalytic effect, isomerization, and aromatization.

[0085] Table 7 Effect of reaction temperature and ethylene pressure on the catalytic performance of MIL-101(Cr)-NS

[0086]

[0087] Reaction conditions: catalyst: MIL-101(Cr)-NS8, 10 μmol (based on MOFs), 1 hour, toluene as solvent, GC determination.

[0088] The present invention has been described in detail above. It will be apparent to those skilled in the art that the present invention may be implemented in a wide range under equivalent parameters, concentrations and conditions without departing from the spirit and scope of the present invention and without the need for unnecessary experimentation. Although the present invention provides specific embodiments, it should be understood that further improvements may be made to the present invention. In short, according to the principles of the present invention, this application intends to include any changes, uses or improvements to the present invention, including changes made by conventional techniques known in the art that depart from the scope disclosed in this application. Applications of some of the basic features may be made within the scope of the following appended claims.

Claims

1. A method for preparing an ethylene polymerization reaction MOFs catalyst, comprising the following steps: modifying a metal organic framework material (MOFs) with sulfonic acid to obtain.

2. The preparation method according to claim 1, characterized in that: The metal organic framework material is MOFs with unsaturated metal Lewis acid sites; preferably at least one of the following: MIL-101(Cr), MIL-101(Cr)-NH2, UiO-66-NH2.

3. The preparation method according to claim 1 or 2, characterized in that: The modification agent used in the sulfonic acid modification is aminosulfonic acid (SA) or 1,3-propanethiol.

4. The preparation method according to claim 3, characterized in that: MIL-101(Cr) was modified with sulfonic acid using aminosulfonic acid as the modifying agent; The specific modification method is as follows: dissolving aminosulfonic acid in deionized water, and then adding MIL-101(Cr) thereto; vigorously stirring the obtained suspension for 2-6 hours, and immersing for 8-16 hours to obtain SA / MIL-101(Cr); Preferably, the mass percentage of the aminosulfonic acid to MIL-101(Cr) is x%, and the value range of x% is 0%-90%, preferably 10%-30%.

5. The preparation method according to claim 3, characterized in that: UiO-66-NH2 was modified with sulfonic acid, and the modification reagent used was 1,3-propanethiol; The specific modification method is as follows: UiO-66-NH2 is dispersed in dichloromethane, and a certain mole of 1,3-propanethiol is added; then the mixture is slowly stirred at 0-40°C for 8-16 hours to obtain UiO-66-NS; Preferably, the feed molar ratio of 1,3-propanethiol to UiO-66-NH2 is x, and the value range of x is 0-8, more preferably 4-8.

6. The preparation method according to claim 3, characterized in that: MIL-101(Cr)-NH2 was modified with sulfonic acid using 1,3-propanethiol as the modification agent; The specific modification method is as follows: MIL-101(Cr)-NH2 is dispersed in dichloromethane, and a certain mole of 1,3-propanethiol is added; then the mixture is slowly stirred at 0-40°C for 8-16 hours to obtain MIL-101(Cr)-NS; Preferably, the feed molar ratio of 1,3-propanethiol to MIL-101(Cr)-NH2 is x, and the value range of x is 0-8, more preferably 4-8.

7. An MOFs catalyst for ethylene oligomerization prepared by the method according to any one of claims 1 to 6.

8. Use of the ethylene oligomerization MOFs catalyst according to claim 7 in catalyzing ethylene oligomerization reactions.

9. A method for ethylene oligomerization, comprising the following steps: using the ethylene oligomerization reaction MOFs catalyst according to claim 7 to catalyze the polymerization reaction of ethylene.

10. The method according to claim 9, characterized in that: The temperature of the polymerization reaction is 15° C. to 35° C., and the ethylene pressure is 0.5 to 1.5 MPa; the amount of the catalyst is 10 umoL; and the reaction is carried out in toluene under stirring.

Citation Information

Patent Citations

  • Method for liquid-phase ethylene oligomerization and polymerization in existence of metal organic framework material

    CN104803818A

  • Oligomerization catalyst to alpha-olefins

    CN1051312A

  • Catalyst system for selective oligomerization of ethylene and ethylene oligomerization reaction method

    WO2019113748A1

Cited By

  • Preparation method and application of NH2-UiO-66 encapsulated sulfamic acid

    CN119976950A

  • Preparation method and application of NH2-UiO-66 encapsulating sulfamic acid