Grinding and separating method for titanium concentrate grading production

Through multi-stage magnetic separation, grinding, spinning and impurity removal processes, combined with optimized closed-circuit grinding system parameters, the problem of low utilization rate of vanadium-titanium magnetite resources has been solved, the output and classification efficiency of titanium concentrate have been improved, and the efficiency of ilmenite concentrate has been reduced. Reduce energy consumption and costs, and achieve efficient use of resources.

CN118807958APending Publication Date: 2024-10-22PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411136231.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

In the comprehensive utilization process of vanadium-titanium magnetite, the resource utilization rate is low, especially the insufficient recovery rate of titanium resources, resulting in resource waste, and the energy consumption and cost of the mineral processing plant are high.

Method used

Multi-stage magnetic separation, grinding, spinning and impurity removal processes are adopted to control mineral particle size through magnetic separation, reduce the number of grinding and return materials, set up a secondary impurity removal process to increase the qualified output of titanium concentrate, and optimize the closed-circuit mill Grinding parameters of the ore system to improve classification efficiency.

Benefits of technology

It effectively improves the grinding and classification efficiency, increases the qualified output of titanium concentrate, reduces energy consumption and costs, improves equipment utilization, and achieves efficient use of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807958A_ABST
    Figure CN118807958A_ABST
Patent Text Reader

Abstract

The invention discloses a grinding and separating method, particularly discloses a grinding and separating method for titanium concentrate grading production, and belongs to the technical field of metallurgical production processes. According to the grinding and separating method for titanium concentrate grading production, the grinding and grading efficiency can be effectively improved, and the qualified yield of titanium concentrate is improved. The grinding and separating method comprises at least two stages of magnetic separation, at least one pass of powder grinding, at least two passes of cyclone separation and at least one pass of impurity removal, and finally a titanium concentrate powder sample with the specified particle size and the specified titanium content is obtained through flotation, minerals entering the next procedure after the first-stage magnetic separation are particle materials with the particle size of 0.1-0.18 mm, and the last-stage magnetic separation is a secondary impurity removal procedure arranged before the titanium concentrate is obtained through flotation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a grinding method, in particular to a grinding method used for titanium concentrate separation production, and belongs to the technical field of metallurgical production process. Background Art

[0002] Panxi area is rich in vanadium-titanium magnetite resources, with proven reserves of 93.933×108t and predicted reserves of 30 billiont, of which iron reserves account for 20% of the country, ranking second in the country; titanium reserves (in terms of TiO2) are 428 milliont, accounting for 93% of the country's reserves, ranking first in the world; vanadium reserves (in terms of V2O5) are 10.4786 milliont, accounting for 63% of the country's reserves, ranking third in the world. The development and utilization of vanadium-titanium magnetite resources in Panxi area has been listed as a national key scientific research project. After decades of efforts, a series of major scientific research results have been achieved. However, in the comprehensive utilization of vanadium-titanium magnetite in the Panxi area, there is also a problem of low resource utilization. The recovery rates of iron, vanadium and titanium elements are about 60%, 39% and 10% respectively. Especially for the precious titanium resources, the utilization rate is about 10% to 20% relative to the original ore, resulting in a large waste of resources. This is the most prominent problem in the comprehensive utilization of Panxi vanadium-titanium magnetite.

[0003] Crushing and grinding is the leading process of the ore dressing plant and the last process of material preparation. The quality of the selection operation index depends largely on the quality of the grinding products. According to statistics, the energy consumption of crushing and grinding in the ore dressing plant accounts for about 65% to 75% of the total energy consumption of the ore dressing plant, and the cost accounts for 50% to 70% of the total cost of the ore dressing plant. Therefore, it has great economic and social benefits to correctly select the grinding process, optimize the grinding process parameters, and improve the grinding and classification efficiency. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a grinding and classification method for titanium concentrate selection production which can effectively improve the grinding and classification efficiency and increase the qualified output of titanium concentrate.

[0005] The technical solution adopted to solve the above technical problems is: a grinding method for titanium concentrate selection production, the grinding method includes at least two stages of magnetic separation, at least one pass of grinding, at least two passes of cyclone separation and at least one pass of impurity removal, and finally flotation to obtain a titanium concentrate powder sample with a specified particle size and a specified titanium content.

[0006] Among them, the raw material for the first stage of magnetic separation is the raw material for grinding in the coarse-grained titanium selection process. After the first stage of magnetic separation, the minerals entering the next process are 0.1-0.18mm particle materials. The last stage of magnetic separation is a secondary impurity removal process set before flotation to obtain titanium concentrate.

[0007] Furthermore, the secondary impurity removal is to remove the inferior iron concentrate in the granular mineral through a two-stage magnetic separation process. Before the inferior iron concentrate is removed through the two-stage magnetic separation process, at least one iron removal process is provided to remove the iron concentrate impurities in the granular mineral.

[0008] The preferred embodiment of the above scheme is that after a stage of magnetic separation, the selected materials are subjected to a cyclone spiral classification, and the minerals meeting the specified particle size enter the square box for further classification, while the minerals not meeting the specified particle size enter the closed-circuit grinding system for re-grinding and classification.

[0009] Furthermore, after being graded and separated by the square box, the minerals that meet the specified particle size directly enter the iron removal process, and the minerals that do not meet the specified particle size enter the ultrasonic high-frequency vibration screen for further sorting and grading; after being graded and separated by the ultrasonic high-frequency vibration screen, the minerals that meet the specified particle size directly enter the iron removal process, and the minerals that do not meet the specified particle size enter the simple grinding system for re-grinding and grading.

[0010] The preferred embodiment of the above scheme is that the simple grinding system includes a ball-and-stick dual-purpose mill and a spiral classifier, the material input end of the spiral classifier is respectively connected to the ultrasonic high-frequency vibration screen and the material output end of the ball-and-stick dual-purpose mill, and the material output end of the spiral classifier is respectively connected to the iron removal device and the material input end of the ball-and-stick dual-purpose mill.

[0011] Furthermore, the closed-circuit grinding system includes a ball mill and a cyclone. The coarse-grained minerals fed into the closed-circuit grinding system are re-grinded and returned at least once between the ball mill and the cyclone, and the minerals meeting the specified particle size directly enter the iron removal process through the cyclone.

[0012] The preferred embodiment of the above scheme is that each closed-circuit grinding system comprises two parallel ball-and-stick dual-purpose mills and a spiral classifier, the material output end of each ball-and-stick dual-purpose mill is connected to the spiral classifier, one outlet end of the spiral classifier is connected to the iron removal device, and the other outlet end of the spiral classifier is connected to the material input end of each ball-and-stick dual-purpose mill.

[0013] Furthermore, the classification return sand ratio of the closed-circuit grinding system is calculated and evaluated according to the following formula:

[0014] C=(β-α) / (α-θ)×100%,

[0015] Wherein, α is the content of a certain particle size in the mill discharge, %; β is the content of a certain particle size in the classification overflow, %. The preferred embodiment of the above scheme is that the grinding ratio of the ball-and-rod dual-purpose mill in the closed-circuit grinding system is calculated and evaluated according to the following formula, i=D / d,

[0016] Where D is the average particle size of the feed ore, and d is the average particle size of the discharge ore.

[0017] Furthermore, the grinding parameters of the ball and rod dual-purpose mill in the closed-circuit grinding system are controlled within the following ranges:

[0018] Feeding rate: 60~70kg·h -1 , the grinding concentration is 65-75%, the classifier overflow concentration is 35-45%, and the classifier angle is 22-25°.

[0019] The beneficial effect of the present invention is that the technical solution provided by the present application is to set the grinding method to include at least two stages of magnetic separation, at least one stage of grinding, at least two stages of cyclone separation and at least one stage of impurity removal, and finally obtain the titanium concentrate powder sample of specified particle size and specified titanium content through flotation, and the raw material in the first stage of magnetic separation adopts the raw material for grinding in the coarse-grained titanium selection process, so that the mineral entering the next process after the first stage of magnetic separation is a 0.1-0.18mm particle material, and then the last stage of magnetic separation is set as a secondary impurity removal process before flotation to obtain titanium concentrate. In this way, since the particle size of the mineral entering the next process is controlled by a first stage of magnetic separation, the number of subsequent grinding passes and the number of returned materials are effectively reduced, thereby achieving the purpose of effectively improving the grinding and classification efficiency, and at the same time, a secondary impurity removal process using magnetic separation as a means is arranged before the final flotation to remove the inferior iron concentrate that still remains in the powder material after the first stage of impurity removal, thereby effectively improving the qualified output of titanium concentrate. Since the grinding and classification method of the present application controls the particle size of the minerals entering the entire process through a stage of magnetic separation, the purpose of reducing the number of grinding and returning materials is achieved, and at the same time, the processing capacity of the ball mill and classification equipment can be effectively released. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a simplified flow chart of the grinding method for titanium concentrate separation production. DETAILED DESCRIPTION

[0021] like Figure 1 The present invention provides a grinding method for titanium concentrate separation production, which can effectively improve the grinding and classification efficiency and increase the qualified output of titanium concentrate. The grinding method includes at least two stages of magnetic separation, at least one pass of powder grinding, at least two passes of cyclone separation and at least one pass of impurity removal, and finally obtains a titanium concentrate powder sample with a specified particle size and a specified titanium content through flotation.

[0022] Among them, the raw material of the first magnetic separation is the raw material for grinding in the coarse-grained titanium selection process, and the minerals entering the next process after the first magnetic separation are 0.1-0.18mm particle materials, and the last magnetic separation is a secondary impurity removal process set before flotation to obtain titanium concentrate. The technical solution provided by the present application is to set the grinding method to include at least two stages of magnetic separation, at least one pass of powder grinding, at least two passes of cyclone separation and at least one pass of impurity removal, and finally obtain the titanium concentrate powder sample of specified particle size and specified titanium content through flotation, and the raw material of the first magnetic separation is the raw material for grinding in the coarse-grained titanium selection process, so that the minerals entering the next process after the first magnetic separation are 0.1-0.18mm particle materials, and then the last magnetic separation is set as a secondary impurity removal process set before flotation to obtain titanium concentrate. In this way, since the particle size of the minerals entering the next process is controlled through a magnetic separation, the number of subsequent grinding passes and the number of returned materials are effectively reduced, thereby achieving the purpose of effectively improving the grinding and classification efficiency. At the same time, a secondary impurity removal process using magnetic separation is arranged before the final flotation to remove the inferior iron concentrate remaining in the powder material after the primary impurity removal, thereby effectively increasing the qualified output of titanium concentrate. Since the grinding and classification method of the present application controls the particle size of the minerals entering the entire process through a magnetic separation, the purpose of reducing the number of grinding and returned materials is achieved, and at the same time, the processing capacity of the ball mill and classification equipment can be effectively released.

[0023] Accordingly, in order to maximize the qualified output of titanium concentrate, the secondary impurity removal of the present application is to remove the inferior iron concentrate in the granular minerals through the two-stage magnetic separation process. Before removing the inferior iron concentrate through the two-stage magnetic separation process, at least one iron removal process is provided to remove the impurities of the iron concentrate in the granular minerals. At the same time, in order to minimize over-grinding, reduce the number of grinding passes and improve the quality of the returned materials, the selected materials after the first stage of magnetic separation of the present application are subjected to a cyclone spiral classification, and the minerals that meet the specified particle size enter the square box for re-classification, and the minerals that do not meet the specified particle size enter the closed-circuit grinding system for re-grinding and classification. After the square box classification and separation, the minerals that meet the specified particle size directly enter the iron removal process, and the minerals that do not meet the specified particle size enter the ultrasonic high-frequency vibration screen for re-selection and classification; after the ultrasonic high-frequency vibration screening classification, the minerals that meet the specified particle size directly enter the iron removal process, and the minerals that do not meet the specified particle size enter the simple grinding system for re-grinding and classification.

[0024] Combined with the existing technology, in order to select the existing general grinding and classification equipment as much as possible, the simple grinding system of the present application includes a ball-and-stick dual-purpose mill and a spiral classifier, the material input end of the spiral classifier is respectively connected to the ultrasonic high-frequency vibration screen and the material output end of the ball-and-stick dual-purpose mill, and the material output end of the spiral classifier is respectively connected to the iron removal device and the material input end of the ball-and-stick dual-purpose mill. The closed-circuit grinding system of the present application includes a ball mill and a cyclone. The coarse-grained minerals fed into the closed-circuit grinding system are re-grinded and returned to the sand at least once between the ball mill and the cyclone, and the minerals that meet the specified particle size directly enter the iron removal process through the cyclone. At the same time, in order to improve the grinding efficiency, each closed-circuit grinding system of the present application includes two parallel ball-and-stick dual-purpose grinding machines and a spiral classifier, the material output end of each ball-and-stick dual-purpose grinding machine is connected to the spiral classifier, one outlet end of the spiral classifier is connected to the iron removal device, and the other outlet end of the spiral classifier is connected to the material input end of each ball-and-stick dual-purpose grinding machine. The preferred method is that the grinding parameters of the ball-and-stick dual-purpose grinding machine of the closed-circuit grinding system are controlled within the following range:

[0025] Feeding rate: 60~70kg·h -1 , the grinding concentration is 65-75%, the classifier overflow concentration is 35-45%, and the classifier angle is 22-25°.

[0026] More specifically, the classification return sand ratio of the closed-circuit grinding system of the present application is calculated and evaluated according to the following formula:

[0027] C=(β-α) / (α-θ)×100%,

[0028] Among them, α is the content of a certain particle size in the mill discharge, %; β is the content of a certain particle size in the classification overflow, %. The grinding ratio of the ball and rod dual-purpose mill in the closed-circuit grinding system is calculated and evaluated according to the following formula:

[0029] i=D / d,

[0030] Where D is the average particle size of the feed ore, and d is the average particle size of the discharge ore.

[0031] To sum up, the above-mentioned grinding method of the present invention solves the problems of low utilization rate of vanadium and titanium resources and low output of titanium concentrate in Panzhihua area; and this invention actively responds to the national call for energy conservation and emission reduction, green production, and strives to achieve "carbon peak and carbon neutrality", and solves the problems of low-carbon, environmental protection, energy reduction, cost reduction, efficiency improvement and development promotion.

[0032] After evaluation, the grinding method of this application produces the following technical effects:

[0033] 1. By designing new production processes, the production capacity of titanium concentrate can be greatly released, thereby promoting the improvement of titanium concentrate operation rate;

[0034] 2. Making full use of the effective production space can greatly improve the utilization rate of equipment and bring out the best performance of equipment;

[0035] 3. The use of combined technology separates the pre-screening and inspection screening of the high-frequency vibrating screen to improve the grading efficiency.

[0036] The technical solution of the present application is further described below through specific embodiments:

[0037] Embodiment 1

[0038] The present invention discloses a method for increasing the output of titanium concentrate, which is achieved by 1) improving the production process; 2) adjusting equipment parameters, etc. The method improves the grinding and classification efficiency in the titanium selection process, releases the processing capacity of the ball mill and the classification equipment, increases the qualified output of titanium concentrate, improves the economic benefits of the enterprise, and is of great significance in energy conservation, emission reduction, cost reduction and efficiency improvement. After the grinding and classification efficiency technology is improved, the grinding and classification cycle load is reduced, the power consumption of the grinding equipment and the classification equipment is reduced, the equipment utilization coefficient is improved, and the grinding output, grinding efficiency, titanium concentrate output and quality are greatly improved.

[0039] The test object selected this time is the raw material for grinding in the coarse-grained titanium selection process of a titanium selection plant in Panxi area. Since the particle size requirement for flotation is below 0.1mm, the evaluation standard for the test results is -0.1mm. According to the requirements of the test plan, the test raw materials were tested and analyzed, and the relevant analysis results are as follows:

[0040]

[0041] As shown in Table 1, the TFe grade of the raw ore entering the mill is 18.30%, and the TiO2 grade is 17.2%, which has a high recycling value. The Ca, Mg, and Al contents (in terms of oxide content) are 10.22%, 9.28%, and 6.50%, respectively, which are relatively high and have a great impact on the subsequent utilization of titanium concentrate.

[0042] In order to better formulate the test plan, a screening test was conducted on the main influencing factors of grinding and classification, namely, the mineral particle size composition. The test equipment mainly used the multi-layer hydraulic screen of the beneficiation and smelting joint laboratory combined with manual inspection and screening. The screening results are shown in Table 2:

[0043]

[0044] From Table 2, we can see that the main particle size of the raw ore entering the mill is concentrated above 150 mesh (0.1mm), and the particle size below 150 mesh accounts for 17.01%, which is coarse. Since the classification particle size is required to be below 0.18mm, the particle size that does not meet the requirements accounts for 58.14%, among which the content between 65-100 mesh is relatively large, and there is a large space available.

[0045] In order to better understand the changes in mineral content between different particle sizes, chemical analysis was performed on the sieve samples of each particle size. The results are as follows:

[0046] As shown in Table 3:

[0047]

[0048]

[0049] From the analysis in Table 3, it can be seen that as the particle size of the raw ore sample decreases, the TFe content and TiO2 content increase. The basic rule is that the finer the particle size, the higher the TFe content and TiO2 content. Among them, when the particle size composition is 150-200 mesh, the TFe and TiO2 contents are 22.35% and 23.26%, respectively, reaching the peak value. And the particle size meets the requirements of the subsequent coarse particle flotation operation of the titanium beneficiation plant, indicating that the grinding classification test should mainly consider the proportion of 150-200 mesh, which can improve the titanium beneficiation operation rate and increase the output of titanium concentrate.

[0050] According to the analysis of process inspection results, the relevant processes were optimized. The optimized flow chart is as follows: Figure 1 shown.

[0051] Subsequently, the new process was tested in the laboratory for verification and the equipment parameters were optimized, and the following conclusions were drawn:

[0052] Combined with the previous test results, the raw materials entering the coarse-grained operation area of ​​the titanium beneficiation plant were taken as the research object. The ball-and-rod dual-purpose mill, ultrasonic high-frequency vibration screen, spiral classifier and other equipment in the beneficiation and smelting joint laboratory were used to form a laboratory small-scale grinding and classification system. The ball mill was expanded and continuous test research was carried out to explore the effects of grinding concentration, feed amount, classifier slope and other conditions on the grinding efficiency of the ball mill. The grouping of test conditions is shown in Table 4:

[0053] Table 4 Statistical table of test conditions for each group

[0054] Group No. <![CDATA[Ore feeding amount / kg·h -1 > Grinding concentration / % Classifier overflow concentration / % Grader angle / . Group 1 60 70 35 22 Group 2 70 70 35 25 Group 3 70 70 40 25 Group 4 70 70 45 25 Group 5 70 65 35 25 Group 6 70 75 35 25

[0055] According to the conditions in Table 4, the ball mill expansion continuous test research was carried out, and the test results are shown in Table 5:

[0056]

[0057]

[0058] In order to understand the working effect of the grinding-classification system in detail, the following formulas are used for calculation and evaluation.

[0059] Classification return sand ratio: C = (β-α) / (α-θ) × 100%,

[0060] Grinding ratio of ball mill: i = D average particle size of feed ore / d average particle size of discharge ore,

[0061] In the above formula: α: the content of a certain particle size in the mill discharge, %; β: the content of a certain particle size in the classification overflow, %.

[0062] Table 8 Technical indicators for the effect of expanded testing

[0063] Group No. Grinding ratio Sand return ratio C Grinding efficiency Classification efficiency Group 1 2.44 95.22% 21.29% 12.48% Group 2 2.11 100.00% 16.01% 18.70% Group 3 2.0 83.96% 20.57% 3.46% Group 4 1.94 72.09% 20.54% 10.32% Group 5 2.03 99.80% 20.03% 19.21% Group 6 1.98 100.91% 18.56% 18.88%

[0064] From the analysis of Table 6, we can see that the fourth group has the best sand return effect. At this time, the content of particles above 100 mesh is the largest, which is beneficial to reduce over-grinding of the mill, and the proportion of particles between 100-150 mesh is 28.47%, which is beneficial to the mill re-grinding and subsequent flotation. From Table 7, we can see that the sixth group has the best overflow effect. At this time, the content of particles above 100 mesh is 4.57%, the content between 100-400 mesh is 58.63%, and the content below 400 mesh is 36.79%. This shows that the over-grinding part is less at this time, and the content of particles that are beneficial to subsequent flotation is larger. The experimental conditions of the sixth group are the best experimental conditions.

[0065] According to the results of laboratory expansion and continuity test, industrial tests were carried out, and the conclusions are shown in Table 9:

[0066] Table 9 The statistical results of ball mill grinding effect are as follows

[0067]

[0068] As shown in Table 9, after process transformation and equipment parameter optimization, the parameters such as grinding efficiency and grinding concentration in the grinding system are much better than the original process, and all meet the design indicators. According to the 1% increase in grinding technical efficiency, the average particle size of the mill discharge will be reduced by 1mm, and the titanium concentrate processing capacity will increase by 1%-2%, which can effectively increase the output of titanium concentrate.

[0069] This application uses one XMBL-Φ420×600 wet grid continuous ball and rod dual-purpose mill in the laboratory, one KM-800-4S vibrating screen for screening, one XBSL-1 / 2″ and one XBSL-3 / 4″ vertical sand pump for slurry transportation, and four independently designed and manufactured slurry sedimentation and concentration devices for concentrate and tailings to form a pilot grinding and classification system, and conducts a continuous test study on the ball mill. The relevant test conditions are shown in Table 4. The following Tables 10 and 11 suggest that only the modified parts should be taken, and the other unadjusted parts should be deleted or used as little as possible (for reference) to reduce the risk of leakage.

[0070] Table 10 Technical parameters of on-site grinding and classifying equipment

[0071]

[0072]

[0073] Table 11 Technical commissioning parameters of grinding and classifying equipment

[0074]

[0075] It should be noted that the terms "first", "second" etc. in the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged in appropriate circumstances, so that the embodiments of the present application described here. In the present application, the orientation or positional relationship indicated by the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inside", "outside", "middle", "vertical", "horizontal", "lateral", "longitudinal" etc. are based on the orientation or positional relationship shown in the accompanying drawings.

[0076] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A grinding method for titanium concentrate separation production, characterized in that: The grinding method comprises at least two stages of magnetic separation, at least one stage of grinding, at least two stages of cyclone separation and at least one stage of impurity removal, and finally flotation to obtain a titanium concentrate powder sample with a specified particle size and a specified titanium content. Among them, the raw material for the first stage of magnetic separation is the raw material for grinding in the coarse-grained titanium selection process. After the first stage of magnetic separation, the minerals entering the next process are 0.1-0.18mm particle materials. The last stage of magnetic separation is a secondary impurity removal process set before flotation to obtain titanium concentrate.

2. The grinding method for titanium concentrate separation production according to claim 1 is characterized in that: The secondary impurity removal is to remove the inferior iron concentrate in the granular mineral through a two-stage magnetic separation process. Before the inferior iron concentrate is removed through the two-stage magnetic separation process, at least one iron removal process is provided to remove the iron concentrate impurities in the granular mineral.

3. The grinding method for titanium concentrate separation production according to claim 1 or 2, characterized in that: After the first stage of magnetic separation, the selected materials are subjected to a cyclone spiral classification. The minerals that meet the specified particle size enter the square box for further classification, and the minerals that do not meet the specified particle size enter the closed-circuit grinding system for re-grinding and classification.

4. The grinding method for titanium concentrate separation production according to claim 3 is characterized in that: After square box grading and separation, the minerals that meet the specified particle size directly enter the iron removal process, and the minerals that do not meet the specified particle size enter the ultrasonic high-frequency vibration screen for further sorting and grading; after ultrasonic high-frequency vibration screening and grading, the minerals that meet the specified particle size directly enter the iron removal process, and the minerals that do not meet the specified particle size enter the simple grinding system for re-grinding and grading.

5. The grinding method for titanium concentrate separation production according to claim 4 is characterized in that: The simple grinding system includes a ball-and-stick dual-purpose mill and a spiral classifier. The material input end of the spiral classifier is respectively connected to the ultrasonic high-frequency vibration screen and the material output end of the ball-and-stick dual-purpose mill, and the material output end of the spiral classifier is respectively connected to the iron removal device and the material input end of the ball-and-stick dual-purpose mill.

6. The grinding method for titanium concentrate separation production according to claim 3 is characterized in that: The closed-circuit grinding system includes a ball mill and a cyclone. The coarse-grained minerals fed into the closed-circuit grinding system are re-grinded and returned at least once between the ball mill and the cyclone. The minerals that meet the specified particle size enter the iron removal process directly through the cyclone.

7. The grinding method for titanium concentrate separation production according to claim 6 is characterized in that: Each closed-circuit grinding system includes two parallel ball-and-stick dual-purpose mills and a spiral classifier. The material output end of each ball-and-stick dual-purpose mill is connected to the spiral classifier, one outlet end of the spiral classifier is connected to the iron removal device, and the other outlet end of the spiral classifier is connected to the material input end of each ball-and-stick dual-purpose mill.

8. The grinding method for titanium concentrate separation production according to claim 7 is characterized in that: The classification return sand ratio of the closed-circuit grinding system is calculated and evaluated according to the following formula: C=(β-α) / (α-θ)×100%, Among them, α is the content of a certain particle size in the mill discharge, %; β is the content of a certain particle size in the classification overflow, %.

9. The grinding method for titanium concentrate separation production according to claim 7 is characterized in that: The grinding ratio of the ball and rod dual-purpose grinding machine in the closed-circuit grinding system is calculated and evaluated according to the following formula: i=D / d, Where D is the average particle size of the feed ore, and d is the average particle size of the discharge ore.

10. The grinding method for titanium concentrate separation production according to claim 7, characterized in that: The grinding parameters of the ball and rod dual-purpose grinding machine in the closed-circuit grinding system are controlled within the following ranges: Feeding rate: 60~70kg·h -1 , the grinding concentration is 65-75%, the classifier overflow concentration is 35-45%, and the classifier angle is 22-25°.

Citation Information

Patent Citations

  • Beneficiation method of low-grade ilmenite

    CN103041912A

  • Recycling process of coarse ilmenite

    CN103433140A

  • Titanium separation method

    CN103706463A

  • Method for producing vanadium-titanium-iron concentrate and ultra-fine particle grade titanium concentrate

    CN114082524A

  • Method for separating high-quality iron ore concentrate from ultralow-grade vanadium titano-magnetite

    CN117983397A