Synchronous powder feeding and swinging laser welding device and method for steel-aluminum dissimilar materials

By using synchronous powder feeding swing laser welding technology in the welding of TRIP high-strength steel and 6061 aluminum alloy, nano-silica powder is used to suppress the generation of aluminum-rich phases, which solves the problem of insufficient mechanical properties of welded joints and achieves efficient connection and simplified processes of welded joints. process.

CN118808901APending Publication Date: 2024-10-22JILIN UNIVERSITY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411125382.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

When the existing technology connects TRIP high-strength steel and 6061 aluminum alloy, the mechanical properties of the welded joint are insufficient, and there are problems such as residual stress concentration after welding, slender nail-shaped welds, and large thickness of Fe-Al intermetallic compounds, resulting in joint failure. The tensile-shear performance is difficult to meet the needs of actual workpiece working conditions, and the commonly used improvement methods increase the complexity and cost of the welding process.

Method used

The synchronous powder feeding swing laser welding method of steel-aluminum dissimilar materials is adopted. Through the inert gas powder feeding device and the laser welder, the sinusoidal swing mode is used to synchronously spray nano-silica powder, and the intersection of the powder and the laser beam is controlled for welding to suppress the aluminum-rich phase. generation to improve the mechanical properties of welded joints.

Benefits of technology

It effectively reduces the thickness of the aluminum-rich phase in the welded joint, increases the connection area and tensile-shear performance of steel-aluminum welding, simplifies the welding process, reduces the concentration of residual stress after welding, and significantly improves the mechanical properties of the welded joint.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118808901A_ABST
    Figure CN118808901A_ABST
Patent Text Reader

Abstract

The invention discloses a steel-aluminum dissimilar material synchronous powder feeding swing laser welding device and method, and the steel-aluminum dissimilar material synchronous powder feeding swing laser welding device comprises an inert gas powder feeding device which is provided with a powder containing tank used for containing nanometer powder to be conveyed; the inert gas cylinder is communicated with the inert gas powder feeding device and is used for containing inert gas; the laser welder is used for emitting a laser beam; a laser head of the laser welder is mounted on the robot arm; the powder feeding nozzle mounting frame is fixedly mounted on the laser head; two nozzle connecting sleeves are arranged on the powder feeding nozzle mounting frame and located on the two sides of the laser head correspondingly. The two powder feeding nozzles communicate with the powder containing tank, and the two powder feeding nozzles are connected into the nozzle connecting sleeves in a one-to-one correspondence mode; and powder outlets of the two powder feeding nozzles face the intersection of the laser beam and the to-be-welded plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser welding of dissimilar materials, and in particular relates to a synchronous powder feeding and swinging laser welding device and method for steel-aluminum dissimilar materials. Background Art

[0002] With the rapid development of the automobile industry and the rise of new energy vehicles, automobile lightweighting and diversification of body materials have become new trends in the development of the automobile industry. In order to reduce the weight of the body, 6061 aluminum alloy with low density, good thermal stability, excellent formability and corrosion resistance is the preferred material for body panels, while most of the body parts used for support and anti-collision still need to use higher strength materials. TRIP800 steel in advanced high-strength steel has the characteristics of high strength, good plasticity, and superior energy absorption capacity due to its special mixed ferrite-austenite structure and morphology, so it is suitable for body structural parts. It can be seen that the mixed use of high-strength steel and lightweight aluminum can achieve lightweight while taking into account safety, and the stability of steel / aluminum alloy hybrid joints is the key factor affecting its application. At present, the commonly used methods for connecting dissimilar materials of TRIP high-strength steel and aluminum alloy steel include MIG arc brazing, resistance spot welding, stir friction welding, etc., but these welding methods have problems such as more welding spatter, large deformation, coarse grain structure, wide heat-affected zone, complex operation, and unsightly appearance.

[0003] Laser welding technology has the characteristics of high energy density, fast cooling speed, small heat input, large depth-to-width ratio, small heat-affected zone and small welding deformation, which can effectively reduce the problems of the above welding methods. In addition, laser welding technology is also easy to operate, highly automated, highly precise, and because it is not contact welding, the wear and deformation of the laser welding machine can be minimized. However, after using the conventional linear laser welding method to connect TRIP high-strength steel and 6061 aluminum alloy, there is still a problem of large accumulation of residual stress on the weld after welding, making it difficult for the tensile shear performance of the welded joint to meet the actual workpiece working conditions. At the same time, the linear laser welding method of TRIP high-strength steel / 6061 aluminum alloy obtains a slender nail-shaped weld. The steel-aluminum spreading area in the TRIP high-strength steel / 6061 aluminum alloy welded joint is limited. The slender nail-shaped weld makes it impossible to significantly improve the mechanical properties of the joint, thereby limiting the mechanical properties of the TRIP high-strength steel / 6061 aluminum alloy laser welded joint.

[0004] In addition, due to the huge differences in thermophysical properties such as melting point, thermal conductivity and thermal expansion coefficient between steel and aluminum, defects such as cracks, pores and fusion difficulties often occur during welding, and a large number of Fe-Al intermetallic compounds (IMCs) will be generated in the joint. The formation of IMCs phase mainly depends on Gibbs free energy. The Fe2Al5 phase with low Gibbs free energy is formed first at the interface, so it is easy to obtain a thicker Fe2Al5 phase. When the aluminum-rich IMCs are thicker, the plasticity and ductility of the welded joint will be significantly reduced, making the joint more prone to cracking. Therefore, suppressing the thickness of brittle phases such as Fe2Al5 and FeAl3 is the key to improving the mechanical properties of the welded joint. In order to suppress the formation of aluminum-rich phases such as FeAl2, Fe2Al5 and FeAl3, the common method is to place metal foil or pre-set powder between the steel and aluminum interlayers, and to suppress the formation of aluminum-rich phases by adding other elements, thereby achieving the purpose of improving the mechanical properties of steel-aluminum welded joints. Placing metal foil between steel and aluminum will cause steel, metal foil and aluminum alloy to react with each other. Different metal foils and steel and aluminum may form other brittle compounds, which will not significantly improve the mechanical properties of steel-aluminum laser welded joints. In addition, adding metal foil between steel and aluminum also needs to consider the effect of its thermal conductivity on weld formation, as well as the waste of excess metal foil in non-welding areas. Placing powder between steel and aluminum will cause problems such as uneven powder placement and gaps between steel and aluminum. The existence of these problems greatly increases the complexity of the laser welding process while using third-party elements to improve the mechanical properties of laser welded joints. At the same time, the increase in process flow is not conducive to the application of steel-aluminum laser welding in actual industrial production. Therefore, it is of great practical significance to simplify the welding process to adapt to automated industrial production while improving the mechanical properties of steel-aluminum laser welded joints. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a steel-aluminum dissimilar material synchronous powder feeding swing laser welding method, which can simplify the welding process of welding steel plates and aluminum alloy plates and improve the mechanical properties of the welded joints.

[0006] The present invention also provides a steel-aluminum dissimilar material synchronous powder feeding swing laser welding device, which can ensure the stability of the powder feeding position and the uniformity of the powder feeding, and further improve the mechanical properties of the welded joint.

[0007] The technical solution provided by the present invention is:

[0008] A steel-aluminum dissimilar material synchronous powder feeding swing laser welding method, comprising:

[0009] An inert gas powder feeding device, which has a powder placing tank for placing the nano powder to be transported;

[0010] an inert gas cylinder, which is connected to the inert gas powder feeding device and is used to contain inert gas;

[0011] A laser welder, which is used to emit a laser beam; the laser head of the laser welder is installed on the robot arm;

[0012] A powder feeding nozzle mounting bracket is fixedly mounted on the laser head; the powder feeding nozzle mounting bracket is provided with two nozzle connecting sleeves, and the two nozzle connecting sleeves are respectively located on both sides of the laser head;

[0013] Two powder delivery nozzles, which are respectively connected to the powder placement tank, and the two powder delivery nozzles are connected to the nozzle connection sleeve in a one-to-one correspondence;

[0014] Wherein, the powder outlets of the two powder feeding nozzles are arranged toward the intersection of the laser beam and the plate to be welded.

[0015] Preferably, the two powder feeding nozzles are symmetrically arranged on both sides of the laser head.

[0016] A steel-aluminum dissimilar material synchronous powder feeding swing laser welding method, using the steel-aluminum dissimilar material synchronous powder feeding swing laser welding device, characterized in that it includes the following steps:

[0017] Step 1: Pre-treating the welding parts of the first plate and the second plate to be welded respectively;

[0018] Wherein, the first plate is a steel plate, and the second plate is an aluminum alloy plate;

[0019] Step 2: overlapping the welding parts of the first plate and the second plate;

[0020] Step 3: welding the overlapped area of ​​the first plate and the second plate by using a laser beam; while welding, spraying nano powder in the form of a powder beam to the intersection of the laser beam and the welding area;

[0021] Wherein, the welding mode is a sinusoidal oscillation mode; the nano powder is silicon powder, and the powder beam moves synchronously with the laser beam.

[0022] Preferably, in step 1, the pretreatment process includes the following steps:

[0023] Step 1: Grind the welding parts of the first plate and the second plate respectively to remove the metal oxide film and burrs on the surface;

[0024] Step 2, placing the polished first plate and the second plate into an ultrasonic instrument containing anhydrous ethanol for cleaning;

[0025] Step 3: After cleaning the first plate and the second plate after ultrasound with acetone, dry them with cold air.

[0026] Preferably, in step three, the welding oscillation frequency is 4 Hz to 8 Hz, the oscillation amplitude is 0.1 mm to 0.5 mm; and the welding speed is 18 mm / s to 22 mm / s.

[0027] Preferably, the welding defocus amount is -2 mm to +2 mm.

[0028] Preferably, the laser welding power is 1500W to 1700W.

[0029] Preferably, the feeding amount of the nano powder is 6.0 g / min.

[0030] Preferably, argon is used as the powder feeding gas.

[0031] Preferably, the particle size of the nano powder is 500nm to 800nm.

[0032] The beneficial effects of the present invention are:

[0033] The steel-aluminum dissimilar materials synchronous powder feeding swinging laser welding method provided by the present invention can synchronously melt nano silicon powder during the welding process. During welding, the molten nano silicon powder enters the unsolidified steel-aluminum welding molten pool and is more evenly distributed inside the molten pool, so that the fluidity between steel and aluminum is improved, and the large-scale enrichment of aluminum elements at the steel-aluminum laser welding interface is suppressed, thereby effectively reducing the thickness of aluminum-rich phases such as Fe2Al5 and FeAl3; avoiding weld defects caused by uneven placement of metal foil or metal powder, simplifying the welding process, and improving the mechanical properties of the welded joint.

[0034] Compared with laser welding in a straight path, the connection width of the steel-aluminum joint in the present invention based on the sinusoidal oscillation mode is increased, which greatly increases the connection area between steel and aluminum.

[0035] Compared with laser welding in a straight path, the longitudinal residual stress distribution on the steel and aluminum laser welding joints changes from being concentrated on the straight line in the center of the weld to being discretely distributed at the peaks and troughs of the sinusoidal oscillation path. The dispersion of residual stress after welding greatly improves the tensile and shear properties of the weldment.

[0036] The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding device provided by the present invention can ensure the stability of the powder feeding position and the uniformity of the powder feeding, and further improve the mechanical properties of the welded joint. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a schematic diagram of the steel-aluminum dissimilar materials synchronous powder feeding swing laser welding device described in the present invention.

[0038] Figure 2 Schematic diagram of the inert gas powder feeding device of the present invention.

[0039] Figure 3 Schematic diagram of the overall structure of the welding system used in the present invention.

[0040] Figure 4 It is a schematic diagram of the moving path of the laser beam in the synchronous powder feeding swinging laser welding method of steel-aluminum dissimilar materials described in the present invention.

[0041] Figure 5 (a) is the macroscopic morphology of the weld obtained by linear laser welding mode.

[0042] Figure 5 (b) is a macroscopic morphology of the weld obtained by using the steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method described in the present invention.

[0043] Figure 6 (a) is a metallographic image of the cross section of the welded joint obtained by using the steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method described in the present invention.

[0044] Figure 6 (b) is a cross-sectional metallographic image of the welded joint obtained by linear laser welding mode. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0046] like Figure 1-2 As shown, the present invention provides a steel-aluminum dissimilar material synchronous powder feeding swing laser welding device, which includes: a laser welder 110, an inert gas powder feeding device 120, a powder feeding nozzle 121, an inert gas cylinder 130, a powder feeding nozzle mounting bracket 140, a nozzle connecting sleeve 141 and a robot arm 150.

[0047] The inert gas powder feeding device 120 has two powder placement tanks 123 for placing the nano powder to be transported. The inert gas cylinder 130 is used to contain inert gas and is connected to the inert gas powder feeding device 120 through a hose. The laser welder 110 is used to emit a laser beam; the laser head of the laser welder 110 is installed on the robot arm 150, and the laser head is connected to the laser generator of the laser welder through a laser fiber connecting tube 111. The powder feeding nozzle mounting frame 140 is fixedly installed on the laser head; the powder feeding nozzle mounting frame 140 is provided with two nozzle connecting sleeves 141, and the two nozzle connecting sleeves 141 are respectively located on both sides of the laser head. The two powder feeding nozzles 121 are respectively connected to the two powder placement tanks 123 through a hose 122, and the two powder feeding nozzles 121 are connected to the nozzle connecting sleeves 141 one by one. The first plate (steel plate) 210 and the second plate 220 (aluminum alloy thin plate) 220 are welded in an overlapping placement form. The second plate (aluminum alloy sheet) 220 is placed on the workbench, located in the lower layer, and the first plate (steel plate) 210 is overlapped on the second plate 220 (aluminum alloy sheet). In order to ensure that the first plate (steel plate) 210 is in a horizontal state when fixed, a heightening gasket 230 of the same material as the first plate (steel plate) 210 is placed between the first plate (steel plate) 210 and the workbench, and then the sample to be welded is fixed with a clamp. Among them, the powder outlets of the two powder feeding nozzles 121 are arranged toward the intersection of the laser beam and the position to be welded, so that the nano powder beam and the laser beam ejected by the inert gas powder feeding device 120 converge at the welding position. The inert gas flow rate can be adjusted by the inert gas powder feeding device 120, thereby changing the powder feeding amount of the nano powder carried by the inert gas.

[0048] As a preferred embodiment, two powder feeding nozzles 121 are symmetrically arranged on both sides of the laser head to make the distribution of the nano powder more uniform.

[0049] like Figure 3 As shown in the figure, the whole welding system includes a voltage-stabilized power supply system, a laser control computer, a robot control cabinet, a robot program setting computer, a laser welder, a water cooling device, a powder feeding device console, an inert gas cylinder and a workbench. Through program design, after setting the laser motion path, oscillation frequency and oscillation amplitude based on the sine mode on the robot program setting computer, the laser head can move according to the set path driven by the robot arm, and at the same time drive the two powder feeding nozzles to move synchronously with the laser head, realizing the welding process and the welding path. Figure 4 shown.

[0050] The present invention also provides a steel-aluminum dissimilar material synchronous powder feeding swing laser welding method, and the specific implementation process is as follows.

[0051] The welding parts of the first plate (steel plate) 210 and the second plate 210 (aluminum alloy thin plate) 220 to be welded are pretreated: the overlapping surfaces of the first plate (steel plate) 210 and the second plate 210 (aluminum alloy thin plate) 220 are polished with sandpaper to remove the surface metal oxide film and burrs; then the polished first plate (steel plate) 210 and the second plate 210 (aluminum alloy thin plate) are placed in an ultrasonic instrument containing 25°C anhydrous ethanol for cleaning for 3 minutes to remove fine stains on the surface of the weldment; then acetone is used to clean the residual organic matter on the surface of the first plate (steel plate) 210 and the second plate 210 (aluminum alloy thin plate), and the surface is blown dry with cold air from a hair dryer to ensure that there is no metal oxide film, oil stains and moisture in the area to be welded.

[0052] Overlap the welding parts of the first plate (steel plate) 210 and the second plate 210 (aluminum alloy sheet) 220: Place the second plate 220 on the workbench, located at the lower layer, and overlap the first plate (steel plate) 210 on the second plate 220. In order to ensure that the first plate (steel plate) 210 is in a horizontal state when fixed, place the heightening gasket 230 of the same material as the first plate (steel plate) 210 between the first plate (steel plate) 210 and the workbench, and then use the clamp to fix the sample to be welded. Fix the precisely installed clamp on the workbench and adjust the working area of ​​the robot arm to correspond to the welding area.

[0053] Adjust the welding parameters of the laser synchronous melting nano powder welding device based on sinusoidal oscillation, set the laser welding power, welding speed, oscillation frequency, oscillation amplitude and powder feeding amount, and perform sinusoidal oscillation laser welding on the overlapping area of ​​the first plate (steel plate) 210 and the second plate 210 (aluminum alloy thin plate) 220. The specific welding parameters are: welding power is 1500W~1700W; welding speed is 18mm / s~22mm / s; defocus is -2mm~+2mm; laser oscillation frequency is 4Hz~8Hz. The laser oscillation amplitude is 0.1mm~0.5mm, which can be set according to actual welding requirements; nano powder uses silicon powder, and the powder feeding amount is 6.0g / min; because the present invention uses two powder feeding nozzles to feed powder at the same time, the powder feeding amount of a single powder feeding nozzle is 3.0g / min.

[0054] In this embodiment, argon is used as the powder feeding gas, and the powder feeding gas flow rate is set to 15-20 L / min.

[0055] The laser welder, robot arm and inert gas powder feeding device are turned on. The robot arm drives the laser head and two powder feeding nozzles of the laser welder to move along the set welding path to achieve welding of the overlapping area of ​​the first plate and the second plate. Under the irradiation of the high-energy-density laser beam, the nanopowder sprayed onto the welding area is melted synchronously with the weldment to form a laser welding molten pool, thereby greatly improving the connection strength between steel and aluminum dissimilar materials.

[0056] The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method provided by the present invention is further described below in conjunction with specific embodiments and comparative examples.

[0057] The plates, pretreatment methods and fixing methods used in the following embodiments and comparative examples are the same, specifically:

[0058] The first plate: TRIP800 steel plate, size 100×30×1.2mm;

[0059] Second plate: 6061 aluminum alloy sheet, size 100×30×2mm;

[0060] The pretreatment process is as follows: the overlapping surfaces of the 6061 aluminum alloy sheet and the TRIP800 steel plate are polished with 800#, 1500#, and 2000# sandpapers in turn to remove the surface metal oxide film and burrs, and then the TRIP800 steel plate and the 6061 aluminum alloy sheet to be welded are placed in an ultrasonic instrument containing 25°C anhydrous ethanol for cleaning for 3 minutes to remove fine stains on the surface of the weldment, and then acetone is used to clean the residual organic matter on the surface of the TRIP800 steel plate and the 6061 aluminum alloy sheet to be welded and blown dry with cold air from a hair dryer to ensure that there is no metal oxide film, oil stains, and moisture in the area to be welded.

[0061] The fixing method is: overlap the welding parts of the first plate (TRIP800 steel plate) 210 and the second plate 220 (6061 aluminum alloy sheet): place the second plate 220 on the workbench, located in the lower layer, and overlap the first plate (steel plate) 210 on the second plate 220. In order to ensure that the first plate (steel plate) 210 is in a horizontal state during fixing, place the heightening gasket 230 of the same material as the first plate (steel plate) 210 between the first plate (steel plate) 210 and the workbench, and then use the clamp to fix the sample to be welded. Fix the precisely installed clamp on the workbench, and adjust the working area of ​​the robot arm to correspond to the welding area.

[0062] The welding parameters in each embodiment and comparative example and the maximum tensile shear force of the obtained welded joints are shown in Table 1.

[0063] Table 1 Maximum tensile shear force of joints under different welding process parameters

[0064]

[0065]

[0066] In each embodiment and comparative example, the powder feeding amount is set to 6.0 g / min, and the laser swing amplitude is set to 0.3 mm.

[0067] As can be seen from Table 1, Examples 1-9 can improve the mechanical properties of the welded joint by reasonably setting the four welding parameters of oscillation frequency, welding speed, welding power and defocus. When the oscillation frequency is 4Hz-8Hz, the welding speed is 18mm / s-22mm / s, the welding power is 1500W-1700W, and the defocus is in the range of -2mm-+2mm, a relatively impressive joint tensile shear performance can be obtained. Under the optimal welding parameters: laser welding power: 1600W, laser welding speed: 20mm / s, defocus: 0, laser oscillation frequency: 6Hz, powder feeding: 6.0g / min, laser oscillation amplitude: 0.3mm; the tensile shear performance of the welded joint reaches 1722.1N.

[0068] In addition, the weld obtained by the method of the present invention is compared with the weld obtained by straight line welding. Figure 5 As shown in the figure, by comparing the macroscopic morphology of the weld, it can be found that the weld obtained by the continuous laser welding technology based on the sinusoidal oscillation path has a larger weld width than that of the linear welding. Figure 6 As shown in the figure, through the metallographic images of the weld cross-sections of the two, it is found that sinusoidal oscillation welding can increase the spreading area between steel and aluminum, transforming the nail-shaped weld of conventional linear laser welding into a rectangular weld, further increasing the effective connection area of ​​the welded joint of dissimilar materials. Under the optimal welding parameters, the shear strength of the weldment based on conventional laser welding of a linear path is 98.82N / mm, and the shear strength of the weldment based on sinusoidal oscillation laser synchronous melting nano-silicon powder welding is 143.51N / mm, and the shear strength is increased by 45.23%.

[0069] The improvement of tensile shear strength is mainly due to the following three factors:

[0070] (1) Compared with laser welding using a straight path, the connection width of the steel-aluminum joint based on the sinusoidal oscillation mode is increased from 0.53 mm to 1.34 mm, and the connection width is increased by 150.28%, which greatly increases the effective connection area between steel and aluminum.

[0071] (2) Compared with laser welding in a straight path, the longitudinal residual stress distribution on the steel-aluminum laser welding joint changes from being concentrated on the straight line in the center of the weld to being discretely distributed at the peaks and troughs of the sinusoidal oscillation path. The dispersion of residual stress after welding is also one of the reasons for the significant improvement in the tensile shear performance of the weldment.

[0072] (3) By synchronously melting the nano-silicon powder, the molten nano-silicon powder enters the unsolidified steel-aluminum welding pool during welding and is more evenly distributed inside the molten pool, thereby improving the fluidity between steel and aluminum and inhibiting the large-scale enrichment of aluminum elements at the steel-aluminum laser welding interface, thereby effectively reducing the thickness of aluminum-rich phases such as Fe2Al5 and FeAl3, thereby improving the mechanical properties of the joint in terms of microstructural structure.

[0073] The steel-aluminum dissimilar materials synchronous powder feeding swinging laser welding method provided by the present invention increases the connection area of ​​the overlap of the dissimilar materials, and at the same time reduces the concentration of longitudinal residual stress after welding through the welding method of the swing curve path, thereby greatly improving the connection strength between the steel and aluminum dissimilar materials; in addition, through the laser synchronous melting nano powder welding method, the complicated process of pre-setting powder or metal foil before welding is reduced, the automation process of laser welding is optimized, and the welding process is simplified.

[0074] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A synchronous powder feeding swing laser welding device for steel-aluminum dissimilar materials, include: An inert gas powder feeding device, which has a powder placing tank for placing the nano powder to be transported; an inert gas cylinder, which is connected to the inert gas powder feeding device and is used to contain inert gas; A laser welder, which is used to emit a laser beam; the laser head of the laser welder is installed on the robot arm; A powder feeding nozzle mounting bracket is fixedly mounted on the laser head; the powder feeding nozzle mounting bracket is provided with two nozzle connecting sleeves, and the two nozzle connecting sleeves are respectively located on both sides of the laser head; Two powder delivery nozzles, which are respectively connected to the powder placement tank, and the two powder delivery nozzles are connected to the nozzle connection sleeve in a one-to-one correspondence; Wherein, the powder outlets of the two powder feeding nozzles are arranged toward the intersection of the laser beam and the plate to be welded.

2. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding device according to claim 1, It is characterized in that The two powder feeding nozzles are symmetrically arranged on both sides of the laser head.

3. A steel-aluminum dissimilar material synchronous powder feeding swing laser welding method, using the steel-aluminum dissimilar material synchronous powder feeding swing laser welding device as described in any one of claims 1-2, It is characterized in that The steps include: Step 1: Pre-treating the welding parts of the first plate and the second plate to be welded respectively; Wherein, the first plate is a steel plate, and the second plate is an aluminum alloy plate; Step 2: overlapping the welding parts of the first plate and the second plate; Step 3: welding the overlapped area of ​​the first plate and the second plate by using a laser beam; while welding, spraying nano powder in the form of a powder beam to the intersection of the laser beam and the welding area; Wherein, the welding mode is a sinusoidal oscillation mode; the nano powder is silicon powder, and the powder beam moves synchronously with the laser beam.

4. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 3, It is characterized in that In step 1, the pre-processing process includes the following steps: Step 1: Grind the welding parts of the first plate and the second plate respectively to remove the metal oxide film and burrs on the surface; Step 2, placing the polished first plate and the second plate into an ultrasonic instrument containing anhydrous ethanol for cleaning; Step 3: After cleaning the first plate and the second plate after ultrasound with acetone, dry them with cold air.

5. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 4, It is characterized in that In the step three, the welding oscillation frequency is 4 Hz to 8 Hz, the oscillation amplitude is 0.1 mm to 0.5 mm; and the welding speed is 18 mm / s to 22 mm / s.

6. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 5, It is characterized in that The welding defocus range is -2mm to +2mm.

7. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 5 or 6, It is characterized in that The laser welding power is 1500W~1700W.

8. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 7, It is characterized in that The feeding amount of the nano powder is 6.0 g / min.

9. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 8, It is characterized in that Argon was used as the powder feeding gas.

10. The steel-aluminum dissimilar materials synchronous powder feeding swing laser welding method according to claim 9, It is characterized in that The particle size of the nano powder is 500nm-800nm.

Citation Information

Patent Citations

  • Method and apparatus for joining workpieces at a lap joint

    CN107000119A

  • Aluminum-steel dissimilar material laser welding method

    CN112894132A

  • Laser welding system, laser welding control method and device and storage medium

    CN113182686A

  • Dissimilar metal laser cladding welding device and method

    CN114178699A

  • Method for welding dissimilar metallic joining partners

    DE102015009664B3